{"id":20136,"date":"2024-12-30T11:36:00","date_gmt":"2024-12-30T03:36:00","guid":{"rendered":"https:\/\/steelprogroup.com\/?p=20136"},"modified":"2025-01-14T12:00:30","modified_gmt":"2025-01-14T04:00:30","slug":"l6","status":"publish","type":"post","link":"https:\/\/steelprogroup.com\/ar\/tool-steel\/grades\/l6\/","title":{"rendered":"\u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0623\u062f\u0648\u0627\u062a L6 | SKT4 | 1.2713: \u0627\u0644\u062e\u0635\u0627\u0626\u0635 \u0648\u0627\u0644\u0628\u064a\u0627\u0646\u0627\u062a \u0648\u0627\u0644\u0645\u0646\u062a\u062c\u0627\u062a"},"content":{"rendered":"<p class=\"wp-block-paragraph\">\u0641\u064a SteelPro Group\u060c \u0646\u0648\u0641\u0631 \u0645\u0646\u062a\u062c\u0627\u062a \u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0623\u062f\u0648\u0627\u062a L6 \u0639\u0627\u0644\u064a\u0629 \u0627\u0644\u062c\u0648\u062f\u0629 \u0627\u0644\u062a\u064a \u062a\u0644\u0628\u064a \u0627\u0644\u0645\u0639\u0627\u064a\u064a\u0631 \u0627\u0644\u062f\u0648\u0644\u064a\u0629 \u0645\u062b\u0644 ASTM A681 \u0648SAE J437 \u0648J438. \u0645\u0639 \u0623\u0643\u062b\u0631 \u0645\u0646 \u0639\u0642\u062f \u0645\u0646 \u0627\u0644\u062e\u0628\u0631\u0629 \u0648\u0631\u062f\u0648\u062f \u0627\u0644\u0641\u0639\u0644 \u0627\u0644\u0625\u064a\u062c\u0627\u0628\u064a\u0629 \u0645\u0646 \u0627\u0644\u0639\u0645\u0644\u0627\u0621\u060c \u0646\u062d\u0646 \u0634\u0631\u064a\u0643\u0643 \u0627\u0644\u0645\u0648\u062b\u0648\u0642 \u0628\u0647 \u0644\u0644\u062d\u0635\u0648\u0644 \u0639\u0644\u0649 \u062d\u0644\u0648\u0644 \u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0623\u062f\u0648\u0627\u062a \u0627\u0644\u0645\u0648\u062b\u0648\u0642\u0629 \u0648\u0627\u0644\u0645\u062a\u064a\u0646\u0629.<\/p><h2 class=\"wp-block-heading\">\u0645\u0627 \u0647\u0648 \u0627\u0644\u0641\u0648\u0644\u0627\u0630 \u0623\u062f\u0627\u0629 L6\u061f<\/h2><p class=\"wp-block-paragraph\">\u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0623\u062f\u0648\u0627\u062a L6 \u0647\u0648 \u0641\u0648\u0644\u0627\u0630 \u0633\u0628\u0627\u0626\u0643\u064a \u0645\u062a\u0639\u062f\u062f \u0627\u0644\u0627\u0633\u062a\u062e\u062f\u0627\u0645\u0627\u062a \u0648\u0645\u0642\u0648\u0649 \u0628\u0627\u0644\u0632\u064a\u062a. \u064a\u062a\u0645\u062a\u0639 \u0628\u0645\u0642\u0627\u0648\u0645\u0629 \u062c\u064a\u062f\u0629 \u0644\u0644\u0635\u062f\u0645\u0627\u062a \u0628\u0633\u0628\u0628 \u0645\u062d\u062a\u0648\u0627\u0647 \u0627\u0644\u0639\u0627\u0644\u064a \u0645\u0646 \u0627\u0644\u0646\u064a\u0643\u0644. \u064a\u062d\u0627\u0641\u0638 \u0641\u0648\u0644\u0627\u0630 L6 \u0639\u0644\u0649 \u0635\u0644\u0627\u0628\u062a\u0647 \u0627\u0644\u062a\u064a \u062a\u0628\u0644\u063a 60 HRC \u0623\u0648 \u0623\u0639\u0644\u0649 \u0645\u0639 \u0633\u0645\u0643 \u0645\u0642\u0637\u0639 \u064a\u0635\u0644 \u0625\u0644\u0649 75 \u0645\u0645 (3 \u0628\u0648\u0635\u0627\u062a). \u0625\u0646\u0647 \u0645\u062b\u0627\u0644\u064a \u0644\u0644\u0623\u062f\u0648\u0627\u062a \u0648\u0627\u0644\u0642\u0648\u0627\u0644\u0628 \u0648\u0623\u062c\u0632\u0627\u0621 \u0627\u0644\u0622\u0644\u0627\u062a \u0627\u0644\u062a\u064a \u062a\u062a\u0637\u0644\u0628 \u062a\u0648\u0627\u0632\u0646\u064b\u0627 \u0628\u064a\u0646 \u0627\u0644\u0635\u0644\u0627\u0628\u0629 \u0648\u0627\u0644\u0645\u062a\u0627\u0646\u0629 \u0645\u062b\u0644 \u0627\u0644\u0645\u063a\u0627\u0632\u0644 \u0648\u0627\u0644\u0643\u0627\u0645\u0627\u062a \u0648\u0627\u0644\u0645\u0642\u0627\u0628\u0636 \u0648\u0627\u0644\u0645\u062b\u0628\u062a\u0627\u062a.<\/p><p class=\"wp-block-paragraph\">\u064a\u062a\u0645\u064a\u0632 \u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0623\u062f\u0648\u0627\u062a L6 \u0628\u0633\u0647\u0648\u0644\u0629 \u0627\u0644\u062a\u0635\u0646\u064a\u0639\u060c \u062d\u064a\u062b \u064a\u062a\u0645 \u062a\u0635\u0646\u064a\u0641\u0647 \u0639\u0646\u062f 90% \u0645\u0646 \u0627\u0644\u0641\u0648\u0644\u0627\u0630 \u0645\u0646\u062e\u0641\u0636 \u0627\u0644\u0633\u0628\u0627\u0626\u0643 \u0645\u0646 \u0627\u0644\u0645\u062c\u0645\u0648\u0639\u0629 W \u064875% \u0645\u0646 \u0627\u0644\u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0643\u0631\u0628\u0648\u0646\u064a 1%.<\/p><h3 class=\"wp-block-heading\">\u0645\u0627 \u0647\u0648 \u0627\u0644\u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0628\u064a\u0646\u064a\u062a L6\u061f<\/h3><p class=\"wp-block-paragraph\">\u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0628\u0627\u064a\u0646\u064a\u062a L6 \u0647\u0648 \u0623\u062d\u062f \u0623\u0646\u0648\u0627\u0639 \u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0623\u062f\u0648\u0627\u062a L6 \u0627\u0644\u0630\u064a \u064a\u062e\u0636\u0639 \u0644\u0639\u0645\u0644\u064a\u0629 \u0645\u0639\u0627\u0644\u062c\u0629 \u062d\u0631\u0627\u0631\u064a\u0629 \u062a\u062a\u0636\u0645\u0646 \u062a\u0628\u0631\u064a\u062f\u064b\u0627 \u0645\u062a\u062d\u0643\u0645\u064b\u0627 \u0641\u064a\u0647 \u0628\u0639\u062f \u0627\u0644\u0623\u0648\u0633\u062a\u0646\u064a\u062a. \u064a\u062d\u062f\u062b \u0627\u0644\u062a\u062d\u0648\u0644 \u0627\u0644\u0628\u0627\u064a\u0646\u064a\u062a\u064a \u0639\u0627\u062f\u0629\u064b \u0639\u0646\u062f \u062f\u0631\u062c\u0627\u062a \u062d\u0631\u0627\u0631\u0629 \u062a\u062a\u0631\u0627\u0648\u062d \u0628\u064a\u0646 250 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 \u0648550 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (482 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a \u06481022 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a). \u0648\u0628\u0627\u0644\u0645\u0642\u0627\u0631\u0646\u0629 \u0628\u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0645\u0627\u0631\u062a\u0646\u0633\u064a\u062a\u064a L6 \u0627\u0644\u0642\u064a\u0627\u0633\u064a\u060c \u0641\u0625\u0646\u0647 \u064a\u0648\u0641\u0631 \u0635\u0644\u0627\u0628\u0629 \u0648\u0645\u0642\u0627\u0648\u0645\u0629 \u0623\u0639\u0644\u0649 \u0644\u0644\u062a\u0622\u0643\u0644.&nbsp;<\/p><h2 class=\"wp-block-heading\">\u062f\u0631\u062c\u0627\u062a \u0627\u0644\u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0645\u0643\u0627\u0641\u0626\u0629 \u0644\u0640 L6<\/h2><p class=\"wp-block-paragraph\">\u0641\u064a\u0645\u0627 \u064a\u0644\u064a \u0627\u0644\u062c\u062f\u0648\u0644 \u0627\u0644\u0630\u064a \u064a\u062d\u062a\u0648\u064a \u0639\u0644\u0649 \u0627\u0644\u062f\u0631\u062c\u0627\u062a \u0627\u0644\u0642\u064a\u0627\u0633\u064a\u0629 \u0648\u0627\u0644\u0645\u0643\u0627\u0641\u0626\u0629 \u0644\u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0623\u062f\u0648\u0627\u062a L6:<\/p><figure class=\"wp-block-table\"><table><tbody><tr><td><strong>\u0645\u0639\u064a\u0627\u0631<\/strong><\/td><td>\u062c\u064a \u0628\u064a 1299<\/td><td>\u0645\u0639\u0627\u064a\u064a\u0631 ASTM A681<\/td><td>\u062c\u0627\u0645\u0639\u0629 \u0627\u0644\u0623\u0645\u0645 \u0627\u0644\u0645\u062a\u062d\u062f\u0629<\/td><td>\u062f\u064a\u0646 17350<\/td><td>\u0627\u064a\u0632\u0648 4957<\/td><td>\u062c\u064a \u0622\u064a \u0625\u0633 \u062c\u064a 4404<\/td><\/tr><tr><td><strong>\u0627\u0644\u062f\u0631\u062c\u0627\u062a<\/strong><\/td><td>5\u0643\u0631\u0646\u064a\u0645\u0648<\/td><td>\u06446<\/td><td>\u062c\u0627\u0645\u0639\u0629 \u0646\u0628\u0631\u0627\u0633\u0643\u0627 T61206<\/td><td>\u062f\u064a\u0646 1.2713<\/td><td>55\u0646\u064a\u0643\u0644 \u0643\u0631\u0648\u0645 \u0645\u0648\u0628\u064a\u0644 \u0641\u064a7<\/td><td>SKT4<\/td><\/tr><\/tbody><\/table><\/figure><h2 class=\"wp-block-heading\">\u0645\u062c\u0645\u0648\u0639\u0629 \u0623\u0634\u0643\u0627\u0644 \u0648\u062a\u0648\u0631\u064a\u062f\u0627\u062a \u0645\u0646\u062a\u062c\u0627\u062a \u0627\u0644\u0641\u0648\u0644\u0627\u0630 \u0644\u0644\u0623\u062f\u0648\u0627\u062a L6<\/h2><p class=\"wp-block-paragraph\">\u064a\u062a\u0648\u0641\u0631 \u0627\u0644\u0641\u0648\u0644\u0627\u0630 L6 \u0644\u062f\u064a\u0646\u0627 \u0641\u064a \u0645\u062c\u0645\u0648\u0639\u0629 \u0645\u0646 \u0627\u0644\u0623\u0634\u0643\u0627\u0644 \u0627\u0644\u0645\u0633\u062a\u062e\u062f\u0645\u0629 \u0628\u0634\u0643\u0644 \u0634\u0627\u0626\u0639 \u0645\u062b\u0644 \u0627\u0644\u0642\u0636\u0628\u0627\u0646\u060c \u0648\u0627\u0644\u0645\u0633\u0628\u0648\u0643\u0627\u062a\u060c \u0648\u0627\u0644\u0623\u0644\u0648\u0627\u062d\u060c \u0648\u0627\u0644\u062c\u0648\u0644\u0627\u062a\u060c \u0648\u0627\u0644\u0641\u0631\u0627\u063a\u0627\u062a\u060c \u0648\u0627\u0644\u0635\u0641\u0627\u0626\u062d\u060c \u0645\u0639 \u0623\u0628\u0639\u0627\u062f \u0645\u0635\u0645\u0645\u0629 \u0644\u062a\u0644\u0628\u064a\u0629 \u0627\u0644\u0627\u062d\u062a\u064a\u0627\u062c\u0627\u062a \u0627\u0644\u0645\u062d\u062f\u062f\u0629 \u0644\u0639\u0645\u0644\u0627\u0626\u0646\u0627.&nbsp;<\/p><figure class=\"wp-block-table\"><table><tbody><tr><td><strong>\u0646\u0645\u0648\u0630\u062c \u0627\u0644\u0645\u0646\u062a\u062c<\/strong><\/td><td><strong>\u0646\u0637\u0627\u0642 \u0627\u0644\u062d\u062c\u0645 (\u0645\u062a\u0631\u064a)<\/strong><\/td><td><strong>\u0646\u0637\u0627\u0642 \u0627\u0644\u062d\u062c\u0645 (\u0625\u0645\u0628\u0631\u0627\u0637\u0648\u0631\u064a)<\/strong><\/td><\/tr><tr><td rowspan=\"2\">\u0627\u0644\u062d\u0627\u0646\u0627\u062a<\/td><td>\u0627\u0644\u0642\u0637\u0631: 6 \u0645\u0644\u0645 \u0625\u0644\u0649 500 \u0645\u0644\u0645<\/td><td>\u0627\u0644\u0642\u0637\u0631: 0.24 \u0628\u0648\u0635\u0629 \u0625\u0644\u0649 20 \u0628\u0648\u0635\u0629<\/td><\/tr><tr><td>\u0627\u0644\u0637\u0648\u0644: 1000 \u0645\u0644\u0645 \u0625\u0644\u0649 4000 \u0645\u0644\u0645<\/td><td>\u0627\u0644\u0637\u0648\u0644: 40 \u0628\u0648\u0635\u0629 \u0625\u0644\u0649 157 \u0628\u0648\u0635\u0629<\/td><\/tr><tr><td rowspan=\"2\">\u0627\u0644\u0645\u0633\u0628\u0648\u0643\u0627\u062a<\/td><td>\u0627\u0644\u0642\u0637\u0631: 25 \u0645\u0644\u0645 \u0625\u0644\u0649 1200 \u0645\u0644\u0645<\/td><td>\u0627\u0644\u0642\u0637\u0631: 1 \u0628\u0648\u0635\u0629 \u0625\u0644\u0649 47 \u0628\u0648\u0635\u0629<\/td><\/tr><tr><td>\u0627\u0644\u0637\u0648\u0644: 100 \u0645\u0644\u0645 \u0625\u0644\u0649 3000 \u0645\u0644\u0645<\/td><td>\u0627\u0644\u0637\u0648\u0644: \u0645\u0646 4 \u0628\u0648\u0635\u0627\u062a \u0625\u0644\u0649 118 \u0628\u0648\u0635\u0629<\/td><\/tr><tr><td rowspan=\"3\">\u0623\u0637\u0628\u0627\u0642<\/td><td>\u0627\u0644\u0633\u0645\u0643: 5 \u0645\u0644\u0645 \u0625\u0644\u0649 200 \u0645\u0644\u0645<\/td><td>\u0627\u0644\u0633\u0645\u0643: 0.2 \u0628\u0648\u0635\u0629 \u0625\u0644\u0649 7.9 \u0628\u0648\u0635\u0629<\/td><\/tr><tr><td>\u0627\u0644\u0639\u0631\u0636: 100 \u0645\u0644\u0645 \u0625\u0644\u0649 2000 \u0645\u0644\u0645<\/td><td>\u0627\u0644\u0639\u0631\u0636: \u0645\u0646 4 \u0628\u0648\u0635\u0627\u062a \u0625\u0644\u0649 79 \u0628\u0648\u0635\u0629<\/td><\/tr><tr><td>\u0627\u0644\u0637\u0648\u0644: 1000 \u0645\u0644\u0645 \u0625\u0644\u0649 4000 \u0645\u0644\u0645<\/td><td>\u0627\u0644\u0637\u0648\u0644: 40 \u0628\u0648\u0635\u0629 \u0625\u0644\u0649 157 \u0628\u0648\u0635\u0629<\/td><\/tr><tr><td rowspan=\"2\">\u062c\u0648\u0644\u0627\u062a<\/td><td>\u0627\u0644\u0642\u0637\u0631: 10 \u0645\u0644\u0645 \u0625\u0644\u0649 400 \u0645\u0644\u0645<\/td><td>\u0627\u0644\u0642\u0637\u0631: 0.4 \u0628\u0648\u0635\u0629 \u0625\u0644\u0649 15.7 \u0628\u0648\u0635\u0629<\/td><\/tr><tr><td>\u0627\u0644\u0637\u0648\u0644: 1000 \u0645\u0644\u0645 \u0625\u0644\u0649 4000 \u0645\u0644\u0645<\/td><td>\u0627\u0644\u0637\u0648\u0644: 40 \u0628\u0648\u0635\u0629 \u0625\u0644\u0649 157 \u0628\u0648\u0635\u0629<\/td><\/tr><tr><td rowspan=\"3\">\u0627\u0644\u0641\u0631\u0627\u063a\u0627\u062a<\/td><td>\u0627\u0644\u0633\u0645\u0643: 20 \u0645\u0644\u0645 \u0625\u0644\u0649 200 \u0645\u0644\u0645<\/td><td>\u0627\u0644\u0633\u0645\u0643: 0.8 \u0628\u0648\u0635\u0629 \u0625\u0644\u0649 7.9 \u0628\u0648\u0635\u0629<\/td><\/tr><tr><td>\u0627\u0644\u0639\u0631\u0636: 100 \u0645\u0644\u0645 \u0625\u0644\u0649 1000 \u0645\u0644\u0645<\/td><td>\u0627\u0644\u0639\u0631\u0636: \u0645\u0646 4 \u0628\u0648\u0635\u0627\u062a \u0625\u0644\u0649 39 \u0628\u0648\u0635\u0629<\/td><\/tr><tr><td>\u0627\u0644\u0637\u0648\u0644: 100 \u0645\u0644\u0645 \u0625\u0644\u0649 3000 \u0645\u0644\u0645<\/td><td>\u0627\u0644\u0637\u0648\u0644: \u0645\u0646 4 \u0628\u0648\u0635\u0627\u062a \u0625\u0644\u0649 118 \u0628\u0648\u0635\u0629<\/td><\/tr><tr><td rowspan=\"3\">\u0623\u0648\u0631\u0627\u0642<\/td><td>\u0627\u0644\u0633\u0645\u0643: 2 \u0645\u0645 \u0625\u0644\u0649 50 \u0645\u0645<\/td><td>\u0627\u0644\u0633\u0645\u0643: 0.08 \u0628\u0648\u0635\u0629 \u0625\u0644\u0649 2 \u0628\u0648\u0635\u0629<\/td><\/tr><tr><td>\u0627\u0644\u0639\u0631\u0636: 100 \u0645\u0644\u0645 \u0625\u0644\u0649 1500 \u0645\u0644\u0645<\/td><td>\u0627\u0644\u0639\u0631\u0636: \u0645\u0646 4 \u0628\u0648\u0635\u0627\u062a \u0625\u0644\u0649 59 \u0628\u0648\u0635\u0629<\/td><\/tr><tr><td>\u0627\u0644\u0637\u0648\u0644: 1000 \u0645\u0644\u0645 \u0625\u0644\u0649 3000 \u0645\u0644\u0645<\/td><td>\u0627\u0644\u0637\u0648\u0644: 40 \u0628\u0648\u0635\u0629 \u0625\u0644\u0649 118 \u0628\u0648\u0635\u0629<\/td><\/tr><\/tbody><\/table><\/figure><h2 class=\"wp-block-heading\">\u0627\u0644\u062a\u0631\u0643\u064a\u0628 \u0627\u0644\u0643\u064a\u0645\u064a\u0627\u0626\u064a \u0644\u0644\u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0645\u0633\u062a\u062e\u062f\u0645 \u0641\u064a \u0635\u0646\u0627\u0639\u0629 \u0627\u0644\u0623\u062f\u0648\u0627\u062a L6<\/h2><figure class=\"wp-block-table\"><table><tbody><tr><td><strong>\u0639\u0646\u0635\u0631<\/strong><\/td><td><strong>\u062a\u0639\u0628\u064a\u0631<\/strong><\/td><\/tr><tr><td>\u0627\u0644\u0643\u0631\u0628\u0648\u0646 (C)<\/td><td>0.60 &#8211; 0.75 %<\/td><\/tr><tr><td>\u0627\u0644\u0643\u0631\u0648\u0645 (Cr)<\/td><td>0.60 &#8211; 1.2 %<\/td><\/tr><tr><td>\u0627\u0644\u0646\u062d\u0627\u0633 (Cu)<\/td><td>\u2264 0.25 %<\/td><\/tr><tr><td>\u0627\u0644\u062d\u062f\u064a\u062f (Fe)<\/td><td>93.6 &#8211; 97.1 %<\/td><\/tr><tr><td>\u0627\u0644\u0645\u0646\u063a\u0646\u064a\u0632 (Mn)<\/td><td>0.25 &#8211; 0.80 %<\/td><\/tr><tr><td>\u0627\u0644\u0645\u0648\u0644\u064a\u0628\u062f\u064a\u0646\u0648\u0645 (Mo)<\/td><td>\u2264 0.50 %<\/td><\/tr><tr><td>\u0627\u0644\u0646\u064a\u0643\u0644 (Ni)<\/td><td>1.25 &#8211; 2.0 %<\/td><\/tr><tr><td>\u0627\u0644\u0641\u0648\u0633\u0641\u0648\u0631 (P)<\/td><td>\u2264 0.030 %<\/td><\/tr><tr><td>\u0627\u0644\u0633\u064a\u0644\u064a\u0643\u0648\u0646 (Si)<\/td><td>\u2264 0.50 %<\/td><\/tr><tr><td>\u0627\u0644\u0643\u0628\u0631\u064a\u062a (S)<\/td><td>\u2264 0.030 %<\/td><\/tr><tr><td>\u0627\u0644\u0641\u0627\u0646\u0627\u062f\u064a\u0648\u0645 (V)<\/td><td>0.20 &#8211; 0.30 %<\/td><\/tr><\/tbody><\/table><\/figure><h2 class=\"wp-block-heading\">\u0627\u0644\u062e\u0635\u0627\u0626\u0635 \u0627\u0644\u0641\u064a\u0632\u064a\u0627\u0626\u064a\u0629 \u0644\u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0623\u062f\u0627\u0629 L6<\/h2><figure class=\"wp-block-table\"><table><tbody><tr><td><strong>\u0645\u0644\u0643\u064a\u0629<\/strong><\/td><td><strong>\u0627\u0644\u0642\u064a\u0645\u0629 \u0627\u0644\u0645\u062a\u0631\u064a\u0629<\/strong><\/td><td><strong>\u0627\u0644\u0642\u064a\u0645\u0629 \u0627\u0644\u0625\u0645\u0628\u0631\u0627\u0637\u0648\u0631\u064a\u0629<\/strong><\/td><\/tr><tr><td>\u0643\u062b\u0627\u0641\u0629<\/td><td>7.85 \u062c\u0631\u0627\u0645\/\u0633\u06453<\/td><td>0.284 \u0631\u0637\u0644\/\u0628\u0648\u0635\u0629 \u0645\u0643\u0639\u0628\u0629<\/td><\/tr><tr><td>\u0646\u0642\u0637\u0629 \u0627\u0644\u0627\u0646\u0635\u0647\u0627\u0631<\/td><td>1421 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629<\/td><td>2590 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a<\/td><\/tr><tr><td>\u0627\u0644\u0645\u0642\u0627\u0648\u0645\u0629 \u0627\u0644\u0643\u0647\u0631\u0628\u0627\u0626\u064a\u0629<\/td><td>0.30 \u03a9\u00b7\u0645\u0645\u00b2\/\u0645<\/td><td>0.000545 \u03a9\u00b7in\u00b2\/ft<\/td><\/tr><tr><td>\u0627\u0644\u0645\u0648\u0635\u0644\u064a\u0629 \u0627\u0644\u062d\u0631\u0627\u0631\u064a\u0629<\/td><td>34.6 \u0648\u0627\u0637\/\u0645\u062a\u0631 \u0643\u0644\u0641\u0646<\/td><td>240 \u0648\u062d\u062f\u0629 \u062d\u0631\u0627\u0631\u064a\u0629 \u0628\u0631\u064a\u0637\u0627\u0646\u064a\u0629\/\u0633\u0627\u0639\u0629\/\u0642\u062f\u0645 \u0645\u0631\u0628\u0639-\u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a<\/td><\/tr><tr><td>\u062f\u0631\u062c\u0629 \u062d\u0631\u0627\u0631\u0629 \u0627\u0644\u062a\u062d\u0648\u0644<\/td><td>730 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629<\/td><td>1350 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a<\/td><\/tr><\/tbody><\/table><\/figure><p class=\"wp-block-paragraph\">\u064a\u0648\u0636\u062d \u0627\u0644\u062c\u062f\u0648\u0644 \u0627\u0644\u062a\u0627\u0644\u064a \u0623\u0646 \u0645\u0639\u0627\u0645\u0644 \u0627\u0644\u062a\u0645\u062f\u062f \u0627\u0644\u062d\u0631\u0627\u0631\u064a (CTE) \u064a\u062a\u063a\u064a\u0631 \u0645\u0639 \u062f\u0631\u062c\u0629 \u0627\u0644\u062d\u0631\u0627\u0631\u0629.<\/p><figure class=\"wp-block-table\"><table><tbody><tr><td><strong>CTE (\u0645\u062a\u0631\u064a)<\/strong><\/td><td><strong>CTE (\u0625\u0645\u0628\u0631\u0627\u0637\u0648\u0631\u064a)<\/strong><\/td><td><strong>\u0627\u0644\u0645\u0632\u0627\u062c (\u0645\u062a\u0631\u064a)<\/strong><\/td><td><strong>\u0627\u0644\u0645\u0632\u0627\u062c (\u0625\u0645\u0628\u0631\u0627\u0637\u0648\u0631\u064a)<\/strong><\/td><\/tr><tr><td>11.3 \u0645\u064a\u0643\u0631\u0648\u0645\u062a\u0631\/\u0645\u062a\u0631-\u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629<\/td><td>6.28 \u0645\u064a\u0643\u0631\u0648\u0646\/\u0628\u0648\u0635\u0629-\u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a<\/td><td>20.0 \u2013 100 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629<\/td><td>68.0 \u2013 212 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a<\/td><\/tr><tr><td>12.6 \u0645\u064a\u0643\u0631\u0648\u0645\u062a\u0631\/\u0645\u062a\u0631-\u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629<\/td><td>7.00 \u0645\u064a\u0643\u0631\u0648\u0646\/\u0628\u0648\u0635\u0629-\u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a<\/td><td>20.0 \u2013 200 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629<\/td><td>68.0 \u2013 392 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a<\/td><\/tr><tr><td>12.6 \u0645\u064a\u0643\u0631\u0648\u0645\u062a\u0631\/\u0645\u062a\u0631-\u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629<\/td><td>7.00 \u0645\u064a\u0643\u0631\u0648\u0646\/\u0628\u0648\u0635\u0629-\u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a<\/td><td>20.0 \u2013 425 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629<\/td><td>68.0 \u2013 797 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a<\/td><\/tr><tr><td>13.5 \u0645\u064a\u0643\u0631\u0648\u0645\u062a\u0631\/\u0645\u062a\u0631-\u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629<\/td><td>7.50 \u0645\u064a\u0643\u0631\u0648\u0646\/\u0628\u0648\u0635\u0629-\u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a<\/td><td>20.0 \u2013 540 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629<\/td><td>68.0 \u2013 1000 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a<\/td><\/tr><tr><td>13.7 \u0645\u064a\u0643\u0631\u0648\u0645\u062a\u0631\/\u0645\u062a\u0631-\u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629<\/td><td>7.61 \u0645\u064a\u0643\u0631\u0648\u0646\/\u0628\u0648\u0635\u0629-\u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a<\/td><td>20.0 \u2013 650 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629<\/td><td>68.0 \u2013 1200 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a<\/td><\/tr><\/tbody><\/table><\/figure><h2 class=\"wp-block-heading\">\u0627\u0644\u062e\u0635\u0627\u0626\u0635 \u0627\u0644\u0645\u064a\u0643\u0627\u0646\u064a\u0643\u064a\u0629 \u0644\u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0623\u062f\u0648\u0627\u062a L6<\/h2><figure class=\"wp-block-table\"><table><tbody><tr><td><strong>\u0645\u0644\u0643\u064a\u0629<\/strong><\/td><td><strong>\u0627\u0644\u0642\u064a\u0645\u0629 \u0627\u0644\u0645\u062a\u0631\u064a\u0629<\/strong><\/td><td><strong>\u0627\u0644\u0642\u064a\u0645\u0629 \u0627\u0644\u0625\u0645\u0628\u0631\u0627\u0637\u0648\u0631\u064a\u0629<\/strong><\/td><td><strong>\u0645\u0644\u062d\u0648\u0638\u0629<\/strong><\/td><\/tr><tr><td rowspan=\"2\">\u0627\u0644\u0635\u0644\u0627\u0628\u0629 (HRC)<\/td><td>45 &#8211; 46<\/td><td>45 &#8211; 46<\/td><td>\u062a\u0645\u062a \u0645\u0639\u0627\u0644\u062c\u062a\u0647 \u0639\u0646\u062f \u062f\u0631\u062c\u0629 \u062d\u0631\u0627\u0631\u0629 427 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (800 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a)<\/td><\/tr><tr><td>61 &#8211; 62<\/td><td>61 &#8211; 62<\/td><td>\u0643\u0645\u0627 \u062a\u0635\u0644\u0628<\/td><\/tr><tr><td>\u0642\u0648\u0629 \u0627\u0644\u0634\u062f \u0627\u0644\u0642\u0635\u0648\u0649<\/td><td>1950 \u0645\u064a\u062c\u0627 \u0628\u0627\u0633\u0643\u0627\u0644<\/td><td>283000 \u0631\u0637\u0644\/\u0628\u0648\u0635\u0629 \u0645\u0631\u0628\u0639\u0629<\/td><td>\u062a\u0645\u062a \u0645\u0639\u0627\u0644\u062c\u062a\u0647 \u0639\u0646\u062f \u062f\u0631\u062c\u0629 \u062d\u0631\u0627\u0631\u0629 204 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (400 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a)<\/td><\/tr><tr><td>\u0642\u0648\u0629 \u0627\u0644\u0634\u062f\u060c \u0627\u0644\u062e\u0636\u0648\u0639<\/td><td>1910 \u0645\u064a\u062c\u0627 \u0628\u0627\u0633\u0643\u0627\u0644<\/td><td>277000 \u0631\u0637\u0644\/\u0628\u0648\u0635\u0629 \u0645\u0631\u0628\u0639\u0629<\/td><td>\u062a\u0645\u062a \u0645\u0639\u0627\u0644\u062c\u062a\u0647 \u0639\u0646\u062f \u062f\u0631\u062c\u0629 \u062d\u0631\u0627\u0631\u0629 204 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (400 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a)<\/td><\/tr><tr><td>\u0627\u0644\u0627\u0633\u062a\u0637\u0627\u0644\u0629 \u0639\u0646\u062f \u0627\u0644\u0643\u0633\u0631<\/td><td>2.0 %<\/td><td>2.0 %<\/td><td>\u062a\u0645\u062a \u0645\u0639\u0627\u0644\u062c\u062a\u0647 \u0639\u0646\u062f \u062f\u0631\u062c\u0629 \u062d\u0631\u0627\u0631\u0629 204 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (400 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a)<\/td><\/tr><tr><td>\u062a\u0642\u0644\u064a\u0644 \u0627\u0644\u0645\u0633\u0627\u062d\u0629<\/td><td>4.0 %<\/td><td>4.0 %<\/td><td>\u062a\u0645\u062a \u0645\u0639\u0627\u0644\u062c\u062a\u0647 \u0639\u0646\u062f \u062f\u0631\u062c\u0629 \u062d\u0631\u0627\u0631\u0629 204 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (400 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a)<\/td><\/tr><tr><td>\u0645\u0639\u0627\u0645\u0644 \u0627\u0644\u0645\u0631\u0648\u0646\u0629<\/td><td>207 \u062c\u064a\u062c\u0627\u0628\u0627\u0633\u0643\u0627\u0644<\/td><td>30000 \u0643.\u0633.<\/td><td>&#8211;<\/td><\/tr><tr><td>\u0627\u064a\u0632\u0648\u062f \u0625\u0645\u0628\u0627\u0643\u062a \u0623\u0646\u0648\u062a\u0634\u062f<\/td><td>298 \u062c<\/td><td>220 \u0642\u062f\u0645 \u0631\u0637\u0644<\/td><td>\u062a\u0645\u062a \u0645\u0639\u0627\u0644\u062c\u062a\u0647 \u0639\u0646\u062f \u062f\u0631\u062c\u0629 \u062d\u0631\u0627\u0631\u0629 204 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (400 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a)<\/td><\/tr><tr><td>\u0634\u0627\u0631\u0628\u064a \u0625\u0645\u0628\u0627\u0643\u062a (V Notch)<\/td><td>5.00 \u062c<\/td><td>3.69 \u0642\u062f\u0645-\u0631\u0637\u0644<\/td><td>\u062a\u0645\u062a \u0645\u0639\u0627\u0644\u062c\u062a\u0647 \u0639\u0646\u062f \u062f\u0631\u062c\u0629 \u062d\u0631\u0627\u0631\u0629 204 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (400 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a)<\/td><\/tr><tr><td>\u0634\u0627\u0631\u0628\u064a \u0625\u0645\u0628\u0627\u0643\u062a\u060c \u063a\u064a\u0631 \u0645\u0643\u062a\u0645\u0644<\/td><td>284.7 \u062c\u0648\u0644<\/td><td>210.0 \u0642\u062f\u0645-\u0631\u0637\u0644<\/td><td>\u062a\u0645\u062a \u0645\u0639\u0627\u0644\u062c\u062a\u0647 \u0639\u0646\u062f \u062f\u0631\u062c\u0629 \u062d\u0631\u0627\u0631\u0629 177 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (350 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a)<\/td><\/tr><tr><td>\u0627\u0644\u062a\u0622\u0643\u0644 (\u0643\u0645\u0627 \u0647\u0648 \u0645\u062a\u0635\u0644\u0628)<\/td><td>74.8 \u0645\u0645\u00b3<\/td><td>74.8 \u0645\u0645\u00b3<\/td><td>\u0627\u0644\u062e\u0633\u0627\u0631\u0629 \u0628\u0627\u0644\u0645\u0644\u0644\u064a\u0645\u062a\u0631 \u0627\u0644\u0645\u0643\u0639\u0628\u060c ASTM G65<\/td><\/tr><tr><td>\u0627\u0644\u062a\u0622\u0643\u0644 (\u0645\u064f\u0642\u0633\u0651\u0649 \u0639\u0646\u062f 650 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a)<\/td><td>139.1 \u0645\u0644\u0645 \u0645\u0643\u0639\u0628<\/td><td>139.1 \u0645\u0644\u0645 \u0645\u0643\u0639\u0628<\/td><td>\u0627\u0644\u062e\u0633\u0627\u0631\u0629 \u0628\u0627\u0644\u0645\u0644\u0644\u064a\u0645\u062a\u0631 \u0627\u0644\u0645\u0643\u0639\u0628\u060c ASTM G65<\/td><\/tr><\/tbody><\/table><\/figure><h2 class=\"wp-block-heading\">\u0627\u0644\u0645\u0639\u0627\u0644\u062c\u0629 \u0627\u0644\u062d\u0631\u0627\u0631\u064a\u0629 \u0644\u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0623\u062f\u0648\u0627\u062a L6<\/h2><h3 class=\"wp-block-heading\">\u062a\u0634\u0643\u064a\u0644 \u0627\u0644\u0641\u0648\u0644\u0627\u0630 L6<\/h3><p class=\"wp-block-paragraph\">\u0639\u0646\u062f \u062a\u0634\u0643\u064a\u0644 \u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0623\u062f\u0648\u0627\u062a L6\u060c \u0642\u0645 \u0628\u062a\u0633\u062e\u064a\u0646\u0647 \u0628\u064a\u0646 1079 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (1975 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a) \u0648871 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (1600 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a). \u0644\u0627 \u062a\u0642\u0645 \u0628\u0627\u0644\u062a\u0634\u0643\u064a\u0644 \u0639\u0646\u062f \u062f\u0631\u062c\u0629 \u062d\u0631\u0627\u0631\u0629 \u0623\u0642\u0644 \u0645\u0646 843 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (1550 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a). \u0628\u0639\u062f \u0627\u0644\u062a\u0634\u0643\u064a\u0644\u060c \u0627\u062a\u0631\u0643 \u0627\u0644\u0641\u0648\u0644\u0627\u0630 \u064a\u0628\u0631\u062f \u062a\u062f\u0631\u064a\u062c\u064a\u064b\u0627 \u0644\u062a\u062c\u0646\u0628 \u0627\u0644\u062a\u0634\u0648\u0647 \u0648\u0627\u0644\u0625\u062c\u0647\u0627\u062f\u0627\u062a \u0627\u0644\u062f\u0627\u062e\u0644\u064a\u0629.<\/p><h3 class=\"wp-block-heading\">\u0627\u0644\u062a\u0644\u062f\u064a\u0646 \u0644\u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0623\u062f\u0648\u0627\u062a L6<\/h3><p class=\"wp-block-paragraph\">\u0628\u0639\u062f \u0627\u0644\u0645\u0639\u0627\u0644\u062c\u0629 \u0627\u0644\u0633\u0627\u062e\u0646\u0629 \u0648\u0642\u0628\u0644 \u0625\u0639\u0627\u062f\u0629 \u0627\u0644\u062a\u0635\u0644\u0628\u060c \u064a\u062a\u0637\u0644\u0628 \u0627\u0644\u0641\u0648\u0644\u0627\u0630 L6 \u0639\u0645\u0644\u064a\u0629 \u0627\u0644\u062a\u0644\u062f\u064a\u0646. \u0642\u0645 \u0628\u062a\u0633\u062e\u064a\u0646 \u0627\u0644\u0641\u0648\u0644\u0627\u0630 \u0625\u0644\u0649 760 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (1400 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a) \u0648\u0627\u062d\u062a\u0641\u0638 \u0628\u0647 \u0639\u0646\u062f \u0647\u0630\u0647 \u0627\u0644\u062f\u0631\u062c\u0629 \u0644\u0645\u062f\u0629 60 \u062f\u0642\u064a\u0642\u0629 \u0644\u0643\u0644 25 \u0645\u0645 (1 \u0628\u0648\u0635\u0629) \u0645\u0646 \u0627\u0644\u0633\u064f\u0645\u0643.&nbsp;<\/p><p class=\"wp-block-paragraph\">\u062b\u0645 \u0642\u0645 \u0628\u062a\u0628\u0631\u064a\u062f \u0627\u0644\u0641\u0648\u0644\u0627\u0630 \u062a\u062f\u0631\u064a\u062c\u064a\u064b\u0627 \u0641\u064a \u0627\u0644\u0641\u0631\u0646 \u0628\u0645\u0639\u062f\u0644 \u0644\u0627 \u064a\u0632\u064a\u062f \u0639\u0646 28 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (50 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a) \u0641\u064a \u0627\u0644\u0633\u0627\u0639\u0629 \u062d\u062a\u0649 \u064a\u0635\u0644 \u0625\u0644\u0649 538 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (1000 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a)\u060c \u0648\u0627\u0633\u062a\u0645\u0631 \u0641\u064a \u0627\u0644\u062a\u0628\u0631\u064a\u062f \u0625\u0644\u0649 \u062f\u0631\u062c\u0629 \u062d\u0631\u0627\u0631\u0629 \u0627\u0644\u063a\u0631\u0641\u0629 \u0625\u0645\u0627 \u0641\u064a \u0627\u0644\u0641\u0631\u0646 \u0623\u0648 \u0628\u0627\u0644\u0647\u0648\u0627\u0621.<\/p><p class=\"wp-block-paragraph\">\u0625\u0630\u0627 \u0643\u0646\u062a \u0628\u062d\u0627\u062c\u0629 \u0625\u0644\u0649 \u062a\u062d\u0633\u064a\u0646 \u0642\u0627\u0628\u0644\u064a\u0629 \u0627\u0644\u062a\u0634\u063a\u064a\u0644\u060c \u0641\u0646\u0648\u0635\u064a\u0643 \u0628\u0625\u0628\u0642\u0627\u0621 \u0627\u0644\u0641\u0648\u0644\u0627\u0630 \u0639\u0646\u062f \u062f\u0631\u062c\u0629 \u062d\u0631\u0627\u0631\u0629 760 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (1400 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a) \u0644\u0645\u062f\u0629 \u0633\u0627\u0639\u0629 \u0644\u0643\u0644 \u0628\u0648\u0635\u0629 \u0645\u0646 \u0627\u0644\u0633\u064f\u0645\u0643\u060c \u062b\u0645 \u062a\u0628\u0631\u064a\u062f\u0647 \u0628\u0628\u0637\u0621 \u0641\u064a \u0627\u0644\u0641\u0631\u0646 \u0645\u0646 677 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (1250 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a) \u0625\u0644\u0649 760 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (1400 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a) \u0644\u0645\u062f\u0629 8 \u0633\u0627\u0639\u0627\u062a \u0642\u0628\u0644 \u0627\u0644\u062a\u0628\u0631\u064a\u062f \u0628\u0627\u0644\u0647\u0648\u0627\u0621. \u062a\u0642\u0644\u0644 \u0647\u0630\u0647 \u0627\u0644\u0639\u0645\u0644\u064a\u0629 \u0645\u0646 \u0627\u0644\u0635\u0644\u0627\u0628\u0629 \u0625\u0644\u0649 \u062d\u0648\u0627\u0644\u064a 192 HBW.<\/p><h3 class=\"wp-block-heading\">\u062a\u0642\u0648\u064a\u0629 \u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0623\u062f\u0648\u0627\u062a L6<\/h3><h4 class=\"wp-block-heading\"><strong>\u0627\u0644\u062a\u0633\u062e\u064a\u0646 \u0627\u0644\u0645\u0633\u0628\u0642<\/strong><\/h4><p class=\"wp-block-paragraph\">\u0642\u0645 \u0628\u062a\u0633\u062e\u064a\u0646 \u0627\u0644\u0641\u0648\u0644\u0627\u0630 L6 \u062a\u062f\u0631\u064a\u062c\u064a\u064b\u0627\u060c \u0628\u062d\u064a\u062b \u0644\u0627 \u064a\u062a\u062c\u0627\u0648\u0632 204 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (400 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a) \u0641\u064a \u0627\u0644\u0633\u0627\u0639\u0629\u060c \u0625\u0644\u0649 621-677 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (1150-1250 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a). \u0627\u0646\u0642\u0639\u0647 \u0644\u0645\u062f\u0629 30 \u062f\u0642\u064a\u0642\u0629 \u0644\u0643\u0644 25 \u0645\u0645 (1 \u0628\u0648\u0635\u0629) \u0645\u0646 \u0627\u0644\u0633\u064f\u0645\u0643\u060c \u0628\u0627\u0644\u0625\u0636\u0627\u0641\u0629 \u0625\u0644\u0649 15 \u062f\u0642\u064a\u0642\u0629 \u0644\u0643\u0644 25 \u0645\u0645 (1 \u0628\u0648\u0635\u0629) \u0625\u0636\u0627\u0641\u064a\u0629.<\/p><h4 class=\"wp-block-heading\"><strong>\u0627\u0644\u062a\u0633\u062e\u064a\u0646 \u0628\u0627\u0644\u0623\u0648\u0633\u062a\u0646\u064a\u062a (\u0627\u0644\u062a\u0633\u062e\u064a\u0646 \u0628\u062f\u0631\u062c\u0629 \u062d\u0631\u0627\u0631\u0629 \u0639\u0627\u0644\u064a\u0629)<\/strong><\/h4><p class=\"wp-block-paragraph\">\u0628\u0639\u062f \u0627\u0644\u062a\u0633\u062e\u064a\u0646 \u0627\u0644\u0645\u0633\u0628\u0642\u060c \u0642\u0645 \u0628\u062a\u0633\u062e\u064a\u0646 \u0627\u0644\u0641\u0648\u0644\u0627\u0630 \u0625\u0644\u0649 788-816 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (1450-1500 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a) \u0641\u064a \u0641\u0631\u0646 \u0623\u0648 \u062d\u0645\u0627\u0645 \u0645\u0644\u062d. \u0627\u0646\u0642\u0639\u0647 \u0644\u0645\u062f\u0629 30 \u062f\u0642\u064a\u0642\u0629 \u0644\u0633\u0645\u0643 25 \u0645\u0645 (1 \u0628\u0648\u0635\u0629)\u060c \u064815 \u062f\u0642\u064a\u0642\u0629 \u0625\u0636\u0627\u0641\u064a\u0629 \u0644\u0643\u0644 25 \u0645\u0645 (1 \u0628\u0648\u0635\u0629) \u0644\u0627\u062d\u0642\u0629. \u0647\u0630\u0627 \u0623\u0645\u0631 \u0628\u0627\u0644\u063a \u0627\u0644\u0623\u0647\u0645\u064a\u0629 \u0644\u0644\u062a\u0635\u0644\u0628 \u0627\u0644\u0633\u0644\u064a\u0645.<\/p><h4 class=\"wp-block-heading\"><strong>\u0625\u062e\u0645\u0627\u062f<\/strong><\/h4><p class=\"wp-block-paragraph\">\u0642\u0645 \u0628\u062a\u0628\u0631\u064a\u062f \u0627\u0644\u0641\u0648\u0644\u0627\u0630 L6 \u0641\u064a \u0627\u0644\u0632\u064a\u062a \u062d\u062a\u0649 \u064a\u0628\u0631\u062f \u0625\u0644\u0649 66-51 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (150-125 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a). \u0628\u0627\u0644\u0646\u0633\u0628\u0629 \u0644\u0644\u0623\u062c\u0632\u0627\u0621 \u0627\u0644\u062a\u064a \u064a\u0642\u0644 \u062d\u062c\u0645\u0647\u0627 \u0639\u0646 3 \u0628\u0648\u0635\u0627\u062a (76.2 \u0645\u0645)\u060c \u0641\u0625\u0646 \u0627\u0644\u062a\u0628\u0631\u064a\u062f \u0628\u0627\u0644\u0647\u0648\u0627\u0621 \u0623\u0648 \u0627\u0633\u062a\u062e\u062f\u0627\u0645 \u0627\u0644\u063a\u0627\u0632 \u0627\u0644\u0645\u0636\u063a\u0648\u0637 \u0647\u0648 \u062e\u064a\u0627\u0631 \u0644\u0644\u062d\u0635\u0648\u0644 \u0639\u0644\u0649 \u0635\u0644\u0627\u0628\u0629 \u0645\u062a\u0648\u0633\u0637\u0629.<\/p><h3 class=\"wp-block-heading\">\u0645\u0639\u0627\u0644\u062c\u0629 \u0627\u0644\u0641\u0648\u0644\u0627\u0630 L6 \u0641\u064a \u062f\u0631\u062c\u0627\u062a \u062d\u0631\u0627\u0631\u0629 \u0645\u0646\u062e\u0641\u0636\u0629<\/h3><p class=\"wp-block-paragraph\">\u064a\u0645\u0643\u0646 \u0625\u062c\u0631\u0627\u0621 \u0627\u0644\u0645\u0639\u0627\u0644\u062c\u0629 \u0639\u0644\u0649 \u062f\u0631\u062c\u0627\u062a \u062d\u0631\u0627\u0631\u0629 \u0645\u0646\u062e\u0641\u0636\u0629 \u0628\u0637\u0631\u064a\u0642\u062a\u064a\u0646:<\/p><ul class=\"wp-block-list\"><li><strong>\u0628\u0639\u062f \u0627\u0644\u0623\u0648\u0633\u062a\u0646\u064a\u062a \u0648\u0627\u0644\u0625\u0637\u0641\u0627\u0621<\/strong>:\u064a\u0633\u0627\u0639\u062f \u0647\u0630\u0627 \u0639\u0644\u0649 \u062a\u062d\u0642\u064a\u0642 \u0635\u0644\u0627\u0628\u0629 \u0645\u0648\u062d\u062f\u0629 \u0648\u064a\u0642\u0644\u0644 \u0627\u0644\u0636\u063a\u0648\u0637 \u0627\u0644\u062f\u0627\u062e\u0644\u064a\u0629 \u0641\u064a \u0648\u0642\u062a \u0645\u0628\u0643\u0631 \u0645\u0646 \u0639\u0645\u0644\u064a\u0629 \u0627\u0644\u0645\u0639\u0627\u0644\u062c\u0629 \u0627\u0644\u062d\u0631\u0627\u0631\u064a\u0629.<\/li>\n\n<li><strong>\u0628\u0639\u062f \u0627\u0644\u062a\u0644\u0637\u064a\u0641<\/strong>:\u064a\u0645\u0643\u0646 \u0623\u0646 \u062a\u0639\u0645\u0644 \u0647\u0630\u0647 \u0627\u0644\u062e\u0637\u0648\u0629 \u0639\u0644\u0649 \u062a\u062d\u0633\u064a\u0646 \u0627\u0644\u0627\u0633\u062a\u0642\u0631\u0627\u0631 \u0627\u0644\u0623\u0628\u0639\u0627\u062f\u064a \u0648\u062a\u0642\u0644\u064a\u0644 \u0627\u0644\u0636\u063a\u0648\u0637 \u0627\u0644\u062f\u0627\u062e\u0644\u064a\u0629\u060c \u0645\u0645\u0627 \u064a\u062c\u0639\u0644 \u0627\u0644\u0641\u0648\u0644\u0627\u0630 \u0623\u0643\u062b\u0631 \u0627\u0633\u062a\u0642\u0631\u0627\u0631\u064b\u0627 \u0644\u0645\u0632\u064a\u062f \u0645\u0646 \u0627\u0644\u0645\u0639\u0627\u0644\u062c\u0629.<\/li><\/ul><p class=\"wp-block-paragraph\">\u064a\u0639\u062a\u0645\u062f \u062a\u0648\u0642\u064a\u062a \u0627\u0644\u0645\u0639\u0627\u0644\u062c\u0629 \u0628\u062f\u0631\u062c\u0627\u062a \u062d\u0631\u0627\u0631\u0629 \u0645\u0646\u062e\u0641\u0636\u0629 \u0639\u0644\u0649 \u0627\u062d\u062a\u064a\u0627\u062c\u0627\u062a\u0643 \u0627\u0644\u0645\u062d\u062f\u062f\u0629 \u0641\u064a\u0645\u0627 \u064a\u062a\u0639\u0644\u0642 \u0628\u0627\u0644\u0627\u0633\u062a\u0642\u0631\u0627\u0631 \u0627\u0644\u0628\u0639\u062f\u064a \u0648\u062a\u062e\u0641\u064a\u0641 \u0627\u0644\u0636\u063a\u0637 \u0627\u0644\u062f\u0627\u062e\u0644\u064a. \u0623\u062e\u0628\u0631\u0646\u0627 \u0625\u0630\u0627 \u0643\u0646\u062a \u0628\u062d\u0627\u062c\u0629 \u0625\u0644\u0649 \u0645\u0633\u0627\u0639\u062f\u0629 \u0641\u064a \u062a\u062d\u062f\u064a\u062f \u0627\u0644\u062d\u0644 \u0627\u0644\u0645\u0646\u0627\u0633\u0628 \u0644\u0645\u0634\u0631\u0648\u0639\u0643.<\/p><h3 class=\"wp-block-heading\">\u062a\u0642\u0633\u064a\u0629 \u0627\u0644\u0641\u0648\u0644\u0627\u0630 L6<\/h3><p class=\"wp-block-paragraph\">\u0628\u0639\u062f \u0627\u0644\u062a\u0628\u0631\u064a\u062f\u060c \u0642\u0645 \u0628\u062a\u0644\u0637\u064a\u0641 \u0627\u0644\u0641\u0648\u0644\u0627\u0630 L6 \u0639\u0644\u0649 \u0627\u0644\u0641\u0648\u0631. \u0642\u0645 \u0628\u0627\u0644\u062a\u0644\u0637\u064a\u0641 \u0639\u0646\u062f 204 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (400 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a) \u0644\u0645\u062f\u0629 \u0633\u0627\u0639\u0629 \u0644\u0643\u0644 \u0628\u0648\u0635\u0629 \u0645\u0646 \u0627\u0644\u0633\u064f\u0645\u0643\u060c \u0645\u0639 \u0636\u0645\u0627\u0646 \u0645\u062f\u0629 \u0644\u0627 \u062a\u0642\u0644 \u0639\u0646 4 \u0633\u0627\u0639\u0627\u062a. \u0627\u062a\u0631\u0643\u0647 \u0644\u064a\u0628\u0631\u062f \u0628\u0634\u0643\u0644 \u0637\u0628\u064a\u0639\u064a \u0625\u0644\u0649 \u062f\u0631\u062c\u0629 \u062d\u0631\u0627\u0631\u0629 \u0627\u0644\u063a\u0631\u0641\u0629.&nbsp;<\/p><p class=\"wp-block-paragraph\">\u0628\u0627\u0644\u0646\u0633\u0628\u0629 \u0644\u0644\u0623\u0642\u0633\u0627\u0645 \u0627\u0644\u0623\u0643\u062b\u0631 \u0633\u0645\u0643\u064b\u0627 (\u0623\u0643\u0628\u0631 \u0645\u0646 6 \u0628\u0648\u0635\u0627\u062a \/ 152.4 \u0645\u0645)\u060c \u0646\u0642\u062a\u0631\u062d \u0627\u0644\u0646\u0642\u0639 \u0644\u0645\u062f\u0629 8-10 \u0633\u0627\u0639\u0627\u062a \u0644\u062a\u0642\u0644\u064a\u0644 \u0627\u0644\u0636\u063a\u0648\u0637 \u0627\u0644\u062f\u0627\u062e\u0644\u064a\u0629 \u0648\u0636\u0645\u0627\u0646 \u0627\u0633\u062a\u0642\u0631\u0627\u0631 \u0623\u0641\u0636\u0644\u060c \u062e\u0627\u0635\u0629\u064b \u0625\u0630\u0627 \u0643\u0627\u0646\u062a \u0623\u062f\u0648\u0627\u062a\u0643 \u0633\u062a\u062e\u0636\u0639 \u0644\u0639\u0645\u0644\u064a\u0629 EDM (\u0627\u0644\u062a\u0635\u0646\u064a\u0639 \u0628\u0627\u0644\u062a\u0641\u0631\u064a\u063a \u0627\u0644\u0643\u0647\u0631\u0628\u0627\u0626\u064a).<\/p><p class=\"wp-block-paragraph\">\u0625\u0630\u0627 \u0643\u0646\u062a \u0628\u062d\u0627\u062c\u0629 \u0625\u0644\u0649 \u0635\u0644\u0627\u0628\u0629 \u0623\u0639\u0644\u0649 \u0639\u0644\u0649 \u062d\u0633\u0627\u0628 \u0628\u0639\u0636 \u0627\u0644\u0635\u0644\u0627\u0628\u0629\u060c \u0641\u0625\u0646 \u0627\u0644\u0645\u0639\u0627\u0644\u062c\u0629 \u0627\u0644\u062d\u0631\u0627\u0631\u064a\u0629 \u0639\u0646\u062f \u062f\u0631\u062c\u0627\u062a \u062d\u0631\u0627\u0631\u0629 \u0623\u0639\u0644\u0649 \u062a\u062a\u0631\u0627\u0648\u062d \u0628\u064a\u0646 232 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 \u0625\u0644\u0649 426 \u062f\u0631\u062c\u0629 \u0645\u0626\u0648\u064a\u0629 (450 \u0625\u0644\u0649 800 \u062f\u0631\u062c\u0629 \u0641\u0647\u0631\u0646\u0647\u0627\u064a\u062a) \u062a\u0639\u0645\u0644 \u0628\u0634\u0643\u0644 \u062c\u064a\u062f. \u0648\u0647\u0630\u0627 \u064a\u0645\u0646\u062d\u0643 \u062a\u0648\u0627\u0632\u0646\u064b\u0627 \u0623\u0641\u0636\u0644 \u0628\u064a\u0646 \u0627\u0644\u0635\u0644\u0627\u0628\u0629 \u0648\u0627\u0644\u0635\u0644\u0627\u0628\u0629 \u0644\u062a\u0637\u0628\u064a\u0642\u0627\u062a \u0645\u0639\u064a\u0646\u0629.<\/p><h2 class=\"wp-block-heading\">\u062a\u0637\u0628\u064a\u0642\u0627\u062a \u0627\u0644\u0641\u0648\u0644\u0627\u0630 \u0644\u0644\u0623\u062f\u0648\u0627\u062a L6<\/h2><p class=\"wp-block-paragraph\">\u064a\u062a\u0645 \u0627\u0633\u062a\u062e\u062f\u0627\u0645 \u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0623\u062f\u0648\u0627\u062a L6 \u0641\u064a \u0627\u0644\u0645\u0648\u0627\u0642\u0641 \u0627\u0644\u062a\u064a \u062a\u062a\u0637\u0644\u0628 \u0627\u0644\u0642\u0648\u0629 \u0648\u0627\u0644\u0645\u062a\u0627\u0646\u0629. \u062a\u0634\u0645\u0644 \u0627\u0644\u0627\u0633\u062a\u062e\u062f\u0627\u0645\u0627\u062a \u0627\u0644\u0634\u0627\u0626\u0639\u0629 \u0645\u0627 \u064a\u0644\u064a:<\/p><ul class=\"wp-block-list\"><li>\u0627\u0644\u0644\u0643\u0645\u0627\u062a \u0648\u0627\u0644\u0642\u0648\u0627\u0644\u0628<\/li>\n\n<li>\u0642\u0648\u0627\u0644\u0628 \u062d\u0642\u0646 \u0627\u0644\u0628\u0644\u0627\u0633\u062a\u064a\u0643<\/li>\n\n<li>\u0627\u0644\u0645\u063a\u0627\u0632\u0644<\/li>\n\n<li>\u0643\u0627\u0645\u064a\u0631\u0627\u062a<\/li>\n\n<li>\u0627\u0644\u0645\u0642\u0627\u0628\u0636 \u0648\u0627\u0644\u0645\u0634\u0627\u0628\u0643<\/li>\n\n<li>\u0623\u062f\u0648\u0627\u062a \u0627\u0644\u0642\u0637\u0639<\/li>\n\n<li>\u0623\u062f\u0648\u0627\u062a \u0627\u0644\u062a\u062b\u0628\u064a\u062a \u0648\u0627\u0644\u062a\u062c\u0647\u064a\u0632\u0627\u062a<\/li>\n\n<li>\u062f\u0628\u0627\u0628\u064a\u0633 \u0623\u0633\u0627\u0633\u064a\u0629<\/li><\/ul><h2 class=\"wp-block-heading\">\u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0623\u062f\u0648\u0627\u062a L6 \u0645\u0642\u0627\u0628\u0644 \u0641\u0648\u0644\u0627\u0630 T10<\/h2><p class=\"wp-block-paragraph\">\u0627\u0644\u0641\u0648\u0644\u0627\u0630 L6 \u0639\u0628\u0627\u0631\u0629 \u0639\u0646 \u0633\u0628\u064a\u0643\u0629 \u0645\u0642\u0648\u0627\u0629 \u0628\u0627\u0644\u0632\u064a\u062a \u0645\u0639\u0631\u0648\u0641\u0629 \u0628\u0642\u0648\u062a\u0647\u0627 \u0648\u0645\u0642\u0627\u0648\u0645\u062a\u0647\u0627 \u0644\u0644\u0635\u062f\u0645\u0627\u062a\u060c \u0645\u0645\u0627 \u064a\u062c\u0639\u0644\u0647\u0627 \u0645\u062b\u0627\u0644\u064a\u0629 \u0644\u0644\u0623\u062f\u0648\u0627\u062a \u0645\u062b\u0644 \u0627\u0644\u0644\u0643\u0645\u0627\u062a \u0648\u0627\u0644\u0642\u0648\u0627\u0644\u0628. \u0625\u0646\u0647\u0627 \u062a\u0648\u0641\u0631 \u0645\u0632\u064a\u062c\u064b\u0627 \u0645\u062a\u0648\u0627\u0632\u0646\u064b\u0627 \u0645\u0646 \u0627\u0644\u0635\u0644\u0627\u0628\u0629 \u0648\u0627\u0644\u0645\u062a\u0627\u0646\u0629. \u0627\u0644\u0641\u0648\u0644\u0627\u0630 T10\u060c \u0648\u0647\u0648 \u0645\u0639\u062f\u0646 \u0639\u0627\u0644\u064a \u0627\u0644\u0643\u0631\u0628\u0648\u0646\u060c \u0623\u0643\u062b\u0631 \u0635\u0644\u0627\u0628\u0629 \u0648\u0623\u0643\u062b\u0631 \u0645\u0642\u0627\u0648\u0645\u0629 \u0644\u0644\u062a\u0622\u0643\u0644\u060c \u0645\u0645\u0627 \u064a\u062c\u0639\u0644\u0647 \u0645\u062b\u0627\u0644\u064a\u064b\u0627 \u0644\u0644\u0623\u062f\u0648\u0627\u062a \u0645\u062b\u0644 \u0627\u0644\u0623\u0632\u0627\u0645\u064a\u0644 \u0648\u0627\u0644\u0634\u0641\u0631\u0627\u062a.<\/p><p class=\"wp-block-paragraph\">\u0628\u0627\u062e\u062a\u0635\u0627\u0631\u060c \u0627\u062e\u062a\u0631 L6 \u0644\u0644\u0635\u0644\u0627\u0628\u0629 \u0648T10 \u0644\u0644\u0635\u0644\u0627\u0628\u0629 \u0648\u0645\u0642\u0627\u0648\u0645\u0629 \u0627\u0644\u062a\u0622\u0643\u0644.<\/p><h2 class=\"wp-block-heading\">\u0623\u062f\u0648\u0627\u062a \u0641\u0648\u0644\u0627\u0630\u064a\u0629 \u0645\u062e\u0635\u0635\u0629 \u0645\u0646 \u0646\u0648\u0639 L6 \u0648\u062e\u062f\u0645\u0627\u062a \u0627\u0644\u062e\u0628\u0631\u0627\u0621 \u0645\u0646 \u0623\u062c\u0644\u0643 \u0641\u0642\u0637<\/h2><p class=\"wp-block-paragraph\">\u0646\u062d\u0646 \u0646\u0648\u0641\u0631 \u0627\u0644\u0641\u0648\u0644\u0627\u0630 \u0627\u0644\u0645\u0633\u062a\u062e\u062f\u0645 \u0641\u064a \u0627\u0644\u0623\u062f\u0648\u0627\u062a L6 \u0641\u064a \u0642\u0636\u0628\u0627\u0646 \u0648\u0623\u0644\u0648\u0627\u062d \u0648\u0645\u0637\u0631\u0648\u0642\u0627\u062a \u0648\u062d\u0644\u0642\u0627\u062a\u060c \u0628\u0623\u062d\u062c\u0627\u0645 \u0645\u062e\u0635\u0635\u0629 \u0644\u062a\u0646\u0627\u0633\u0628 \u0627\u062d\u062a\u064a\u0627\u062c\u0627\u062a\u0643. \u0643\u0645\u0627 \u0646\u0642\u062f\u0645 <a href=\"https:\/\/steelprogroup.com\/ar\/tool-steel\/cr12mov\/\">\u0635\u0641\u0627\u0626\u062d \u0648\u0642\u0636\u0628\u0627\u0646 \u0641\u0648\u0644\u0627\u0630\u064a\u0629 D2.<\/a> \u062a\u0634\u0645\u0644 \u0639\u0631\u0648\u0636\u0646\u0627 \u0627\u0644\u0645\u0639\u0627\u0644\u062c\u0629 \u0627\u0644\u062d\u0631\u0627\u0631\u064a\u0629 \u0648\u0627\u0644\u062a\u0634\u0643\u064a\u0644 \u0648\u0627\u0644\u062a\u0634\u063a\u064a\u0644 \u0627\u0644\u0622\u0644\u064a \u0644\u0644\u062a\u0623\u0643\u062f \u0645\u0646 \u0623\u0646 \u0645\u0646\u062a\u062c\u0627\u062a\u0643 \u062a\u0644\u0628\u064a \u0645\u0639\u0627\u064a\u064a\u0631 \u0627\u0644\u062c\u0648\u062f\u0629 \u0627\u0644\u0639\u0627\u0644\u064a\u0629. \u062a\u0648\u0627\u0635\u0644 \u0645\u0639\u0646\u0627 \u0627\u0644\u064a\u0648\u0645 \u0644\u0644\u062d\u0635\u0648\u0644 \u0639\u0644\u0649 \u0627\u0644\u0645\u0646\u062a\u062c\u0627\u062a \u0648\u0627\u0644\u062f\u0639\u0645 \u0627\u0644\u0630\u064a \u062a\u062d\u062a\u0627\u062c\u0647!<\/p>","protected":false},"excerpt":{"rendered":"<p>At SteelPro Group, we supply high-quality L6 tool steel products that meet international standards like ASTM A681, SAE J437, and [&hellip;]<\/p>","protected":false},"author":12,"featured_media":20126,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_acf_changed":false,"_eb_attr":"","rank_math_lock_modified_date":false,"site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"var(--ast-global-color-4)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"categories":[4294,4293],"tags":[],"class_list":["post-20136","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-grades-tool-steel","category-tool-steel"],"acf":[],"_links":{"self":[{"href":"https:\/\/steelprogroup.com\/ar\/wp-json\/wp\/v2\/posts\/20136","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/steelprogroup.com\/ar\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/steelprogroup.com\/ar\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/steelprogroup.com\/ar\/wp-json\/wp\/v2\/users\/12"}],"replies":[{"embeddable":true,"href":"https:\/\/steelprogroup.com\/ar\/wp-json\/wp\/v2\/comments?post=20136"}],"version-history":[{"count":0,"href":"https:\/\/steelprogroup.com\/ar\/wp-json\/wp\/v2\/posts\/20136\/revisions"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/steelprogroup.com\/ar\/wp-json\/wp\/v2\/media\/20126"}],"wp:attachment":[{"href":"https:\/\/steelprogroup.com\/ar\/wp-json\/wp\/v2\/media?parent=20136"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/steelprogroup.com\/ar\/wp-json\/wp\/v2\/categories?post=20136"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/steelprogroup.com\/ar\/wp-json\/wp\/v2\/tags?post=20136"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}