{"id":20020,"date":"2024-12-23T04:13:00","date_gmt":"2024-12-22T20:13:00","guid":{"rendered":"https:\/\/steelprogroup.com\/?p=20020"},"modified":"2024-12-23T15:47:41","modified_gmt":"2024-12-23T07:47:41","slug":"technical-data","status":"publish","type":"post","link":"https:\/\/steelprogroup.com\/ja\/tool-steel\/grades\/h13\/properties\/technical-data\/","title":{"rendered":"H13 | 1.2344 | SKD61 \u5de5\u5177\u92fc\u6280\u8853\u30c7\u30fc\u30bf"},"content":{"rendered":"<p class=\"wp-block-paragraph\">SteelPro Group \u3067\u306f\u3001\u30d0\u30fc\u3001\u30ed\u30c3\u30c9\u3001\u30ab\u30b9\u30bf\u30e0\u5f62\u72b6\u306a\u3069\u3001\u3055\u307e\u3056\u307e\u306a\u5f62\u72b6\u306e H13 \u5de5\u5177\u92fc\u3092\u4f9b\u7d66\u3057\u3066\u3044\u307e\u3059\u3002\u5f53\u793e\u306e H13 \u92fc\u306f\u3001\u713c\u304d\u306a\u307e\u3057\u72b6\u614b\u3068\u786c\u5316\u72b6\u614b\u306e\u4e21\u65b9\u3067\u63d0\u4f9b\u3055\u308c\u3066\u304a\u308a\u3001\u6b63\u78ba\u306a\u5bf8\u6cd5\u3068\u4ed5\u69d8\u3092\u6e80\u305f\u3059\u7cbe\u5bc6\u6a5f\u68b0\u52a0\u5de5\u30b5\u30fc\u30d3\u30b9\u3082\u63d0\u4f9b\u3057\u3066\u3044\u307e\u3059\u3002<\/p><p class=\"wp-block-paragraph\">H13 \u5de5\u5177\u92fc\u306f\u3001\u9ad8\u6e29\u6761\u4ef6\u4e0b\u3067\u512a\u308c\u305f\u6027\u80fd\u3092\u767a\u63ee\u3059\u308b\u3053\u3068\u3067\u77e5\u3089\u308c\u308b\u591a\u7528\u9014\u306e\u71b1\u9593\u52a0\u5de5\u5de5\u5177\u92fc\u3067\u3059\u3002\u30c0\u30a4\u30ab\u30b9\u30c8\u3001\u62bc\u3057\u51fa\u3057\u3001\u304a\u3088\u3073\u71b1\u75b2\u52b4\u3001\u6469\u8017\u3001\u71b1\u5272\u308c\u8010\u6027\u3092\u5fc5\u8981\u3068\u3059\u308b\u305d\u306e\u4ed6\u306e\u7528\u9014\u3067\u5e83\u304f\u4f7f\u7528\u3055\u308c\u3066\u3044\u307e\u3059\u3002\u30d0\u30e9\u30f3\u30b9\u306e\u53d6\u308c\u305f\u5316\u5b66\u7d44\u6210\u3092\u6301\u3064 H13 \u306f\u3001\u9ad8\u6e29\u3067\u3082\u512a\u308c\u305f\u786c\u5ea6\u3001\u976d\u6027\u3001\u5f37\u5ea6\u3092\u767a\u63ee\u3057\u307e\u3059\u3002<\/p><h2 class=\"wp-block-heading\">H13\u5de5\u5177\u92fc\u306e\u5316\u5b66\u7d44\u6210<\/h2><figure class=\"wp-block-table\"><table><tbody><tr><td><strong>\u8981\u7d20<\/strong><\/td><td><strong>C<\/strong><\/td><td><strong>Si<\/strong><\/td><td><strong>\u30e0\u30f3<\/strong><\/td><td><strong>P\uff08\u6700\u5927\uff09<\/strong><\/td><td><strong>S\uff08\u6700\u5927\uff09<\/strong><\/td><td><strong>Cr<\/strong><\/td><td><strong>\u30e2<\/strong><\/td><td><strong>\u4e94<\/strong><\/td><\/tr><tr><td><strong>ASTM A681<\/strong><\/td><td>0.32 &#8211; 0.45<\/td><td>0.80 &#8211; 1.20<\/td><td>0.20 &#8211; 0.50<\/td><td>0.03<\/td><td>0.03<\/td><td>4.75 &#8211; 5.50<\/td><td>1.10 &#8211; 1.75<\/td><td>0.80 &#8211; 1.20<\/td><\/tr><tr><td><strong>17350 \u898f\u683c<\/strong><\/td><td>0.37 &#8211; 0.42<\/td><td>0.90 &#8211; 1.20<\/td><td>0.30 &#8211; 0.50<\/td><td>0.03<\/td><td>0.03<\/td><td>4.80 &#8211; 5.50<\/td><td>1.20 &#8211; 1.50<\/td><td>0.90 &#8211; 1.10<\/td><\/tr><tr><td><strong>GB\/T 1299<\/strong><\/td><td>0.32 &#8211; 0.42<\/td><td>0.80 &#8211; 1.20<\/td><td>0.20 &#8211; 0.50<\/td><td>0.03<\/td><td>0.03<\/td><td>4.75 &#8211; 5.50<\/td><td>1.10 &#8211; 1.75<\/td><td>0.80 &#8211; 1.20<\/td><\/tr><tr><td><strong>JIS G4404<\/strong><\/td><td>0.35 &#8211; 0.42<\/td><td>0.80 &#8211; 1.20<\/td><td>0.25 &#8211; 0.50<\/td><td>0.03<\/td><td>0.03<\/td><td>4.80 &#8211; 5.50<\/td><td>1.00 &#8211; 1.50<\/td><td>0.80 &#8211; 1.15<\/td><\/tr><\/tbody><\/table><\/figure><h2 class=\"wp-block-heading\">H13\u5de5\u5177\u92fc\u306e\u7269\u7406\u7684\u7279\u6027&nbsp;<\/h2><ul class=\"wp-block-list\"><li>H13\u5de5\u5177\u92fc\u306e\u5bc6\u5ea6\/\u6bd4\u91cd: 7.80 g\/cc ( 0.282 lb\/in\u00b3 )<\/li><\/ul><h2 class=\"wp-block-heading\">H13\u5de5\u5177\u92fc\u306e\u71b1\u7279\u6027<\/h2><figure class=\"wp-block-table\"><table><tbody><tr><td><strong>\u71b1\u7279\u6027<\/strong><\/td><td><strong>\u30e1\u30fc\u30c8\u30eb<\/strong><\/td><td><strong>\u6e29\u5ea6<\/strong><\/td><td><strong>\u82f1\u8a9e<\/strong><\/td><td><strong>\u6e29\u5ea6<\/strong><\/td><\/tr><tr><td rowspan=\"3\">CTE\u3001\u7dda\u5f62<\/td><td>11.0 \u00b5m\/m-\u00b0C<\/td><td>25.0 \u2013 95.0 \u00b0C<\/td><td>6.11 \u00b5in\/in-\u00b0F<\/td><td>77.0 \u2013 203 \u00b0F<\/td><\/tr><tr><td>11.5 \u00b5m\/m-\u00b0C<\/td><td>25.0 \u2013 205.0 \u00b0C<\/td><td>6.39 \u00b5in\/in-\u00b0F<\/td><td>77.0 \u2013 401 \u00b0F<\/td><\/tr><tr><td>12.4 \u00b5m\/m-\u00b0C<\/td><td>25.0 \u2013 540.0 \u00b0C<\/td><td>6.89 \u00b5in\/in-\u00b0F<\/td><td>77.0 \u2013 1000 \u00b0F<\/td><\/tr><tr><td>\u6bd4\u71b1\u5bb9\u91cf<\/td><td>0.460 J\/g-\u00b0C<\/td><td>0.000 \u2013 100 \u00b0C<\/td><td>0.110 BTU\/lb-\u00b0F<\/td><td>32.0 \u2013 212 \u00b0F<\/td><\/tr><tr><td rowspan=\"3\">\u71b1\u4f1d\u5c0e\u7387<\/td><td>24.3W\/mK<\/td><td>215\u2103<\/td><td>169 BTU-\u30a4\u30f3\u30c1\/\u6642-ft\u00b2-\u00b0F<\/td><td>419\u00b0F<\/td><\/tr><tr><td>24.3W\/mK<\/td><td>475\u2103<\/td><td>169 BTU-\u30a4\u30f3\u30c1\/\u6642-ft\u00b2-\u00b0F<\/td><td>887 \u00b0F<\/td><\/tr><tr><td>24.4W\/mK<\/td><td>350<\/td><td>169 BTU-\u30a4\u30f3\u30c1\/\u6642-ft\u00b2-\u00b0F<\/td><td>662<\/td><\/tr><\/tbody><\/table><\/figure><h2 class=\"wp-block-heading\">H13\u5de5\u5177\u92fc\u306e\u6a5f\u68b0\u7684\u7279\u6027&nbsp;<\/h2><figure class=\"wp-block-table\"><table><tbody><tr><td><strong>\u30d7\u30ed\u30d1\u30c6\u30a3<\/strong><\/td><td><strong>\u30e1\u30fc\u30c8\u30eb<\/strong><\/td><td><strong>\u30a4\u30f3\u30da\u30ea\u30a2\u30eb<\/strong><\/td><td><strong>\u6e29\u5ea6<\/strong><\/td><\/tr><tr><td>\u786c\u5ea6\uff08HRC\uff09<\/td><td>45 &#8211; 52<\/td><td>45 &#8211; 52<\/td><td>&#8211;<\/td><\/tr><tr><td>\u5f15\u5f35\u5f37\u5ea6\u3001\u6975\u9650<\/td><td>1200 \u2013 1590 MPa<\/td><td>174.0 \u2013 231.0 ksi<\/td><td>20\u00b0C<\/td><\/tr><tr><td>\u5f15\u5f35\u5f37\u5ea6\u3001\u964d\u4f0f\u5f37\u5ea6<\/td><td>1000 \u2013 1380 MPa<\/td><td>145.0 \u2013 200.0 ksi<\/td><td>20\u00b0C<\/td><\/tr><tr><td>\u5f3e\u6027\u4fc2\u6570<\/td><td>207GPa<\/td><td>30 x 10^6 psi<\/td><td>20\u00b0C<\/td><\/tr><tr><td>\u30dd\u30a2\u30bd\u30f3\u6bd4<\/td><td>0.27 &#8211; 0.30<\/td><td>0.27 &#8211; 0.30<\/td><td>20\u00b0C<\/td><\/tr><tr><td>\u52a0\u5de5\u6027<\/td><td>65 &#8211; 70 %<\/td><td>65 &#8211; 70 %<\/td><td>&#8211;<\/td><\/tr><tr><td>\u9762\u7a4d\u306e\u7e2e\u5c0f<\/td><td>50.00%<\/td><td>50.00%<\/td><td>20\u00b0C<\/td><\/tr><\/tbody><\/table><\/figure><ul class=\"wp-block-list\"><li><em>\u63d0\u4f9b\u3055\u308c\u308b\u5024\u306f\u71b1\u51e6\u7406\u306b\u3088\u3063\u3066\u7570\u306a\u308b\u5834\u5408\u304c\u3042\u308a\u307e\u3059\u3002<\/em><\/li><\/ul><h2 class=\"wp-block-heading\">H13 \u5de5\u5177\u92fc\u71b1\u51e6\u7406\u30c7\u30fc\u30bf<\/h2><figure class=\"wp-block-table\"><table><tbody><tr><td><strong>\u71b1\u51e6\u7406<\/strong><\/td><td><strong>\u6e29\u5ea6<\/strong><\/td><td><strong>\u6e29\u5ea6<\/strong><\/td><td><strong>\u786c\u5ea6<\/strong><\/td><\/tr><tr><td>\u30a2\u30cb\u30fc\u30ea\u30f3\u30b0\u6e29\u5ea6<\/td><td>850 \u2013 870 \u00b0C<\/td><td>1560\uff5e1600\u00b0F<\/td><td>HBC: 41 \u2013 52<\/td><\/tr><tr><td>\u786c\u5316\u6e29\u5ea6<\/td><td>995 \u2013 1040 \u00b0C<\/td><td>1820 \u2013 1900 \u00b0F<\/td><td>HBC: 46 \u2013 56<\/td><\/tr><tr><td>\u713c\u623b\u3057\u6e29\u5ea6<\/td><td>540 \u2013 650 \u00b0C<\/td><td>1000\uff5e1200\u00b0F<\/td><td>HBS: \u6700\u5927235<\/td><\/tr><\/tbody><\/table><\/figure><ul class=\"wp-block-list\"><li><em>\u713c\u920d\u306e\u51b7\u5374\u901f\u5ea6\u306f 1 \u6642\u9593\u3042\u305f\u308a 20\u00b0C \u672a\u6e80\u306b\u3059\u308b\u5fc5\u8981\u304c\u3042\u308a\u307e\u3059\u3002<\/em><\/li><\/ul><h3 class=\"wp-block-heading\">\u5178\u578b\u7684\u306a\u713c\u304d\u623b\u3057\u53cd\u5fdc<\/h3><figure class=\"wp-block-table\"><table><tbody><tr><td><strong>\u713c\u623b\u3057\u6e29\u5ea6<\/strong><\/td><td><strong>\u713c\u623b\u3057\u6e29\u5ea6<\/strong><\/td><td><strong>\u786c\u5ea6\uff08HRC\uff09<\/strong><\/td><td><strong>\u30b7\u30e3\u30eb\u30d4\u30fcV\u30ce\u30c3\u30c1&nbsp;<\/strong><\/td><\/tr><tr><td>540\u2103<\/td><td>1000\u00b0F<\/td><td>52<\/td><td>13.57J (10 \u30d5\u30a3\u30fc\u30c8\u30dd\u30f3\u30c9)<\/td><\/tr><tr><td>550\u2103<\/td><td>1050\u00b0F<\/td><td>50<\/td><td>13.57J (10 \u30d5\u30a3\u30fc\u30c8\u30dd\u30f3\u30c9)<\/td><\/tr><tr><td>565\u2103<\/td><td>1100\u00b0F<\/td><td>48<\/td><td>24.44J (18 \u30d5\u30a3\u30fc\u30c8\u30dd\u30f3\u30c9)<\/td><\/tr><tr><td>580\u2103<\/td><td>1150\u00b0F<\/td><td>44<\/td><td>24.44J (18 \u30d5\u30a3\u30fc\u30c8\u30dd\u30f3\u30c9)<\/td><\/tr><\/tbody><\/table><\/figure><h3 class=\"wp-block-heading\">\u786c\u5316\u4e2d\u306e\u30b5\u30a4\u30ba\u306e\u5909\u5316<\/h3><figure class=\"wp-block-table\"><table><tbody><tr><td><strong>\u786c\u5316\u6e29\u5ea6\uff08\u00b0C\uff09<\/strong><\/td><td><strong>\u713c\u304d\u623b\u3057\u6e29\u5ea6 (\u00b0C)<\/strong><\/td><td><strong>\u7e26\u65b9\u5411\u306e\u30b5\u30a4\u30ba\u5909\u66f4\uff08%\uff09<\/strong><\/td><td><strong>\u786c\u5ea6\uff08HRC\uff09<\/strong><\/td><\/tr><tr><td rowspan=\"2\">1010\uff081850\u00b0F\uff09<\/td><td>540\uff081000\u00b0F\uff09<\/td><td>0.07%<\/td><td>52<\/td><\/tr><tr><td>595\uff081100\u00b0F\uff09<\/td><td>0.08%<\/td><td>47<\/td><\/tr><\/tbody><\/table><\/figure><h2 class=\"wp-block-heading\">SteelPro Group H13\u5de5\u5177\u92fc\u3092\u4f7f\u3044\u59cb\u3081\u308b<\/h2><p class=\"wp-block-paragraph\">\u9ad8\u54c1\u8cea\u3092\u304a\u63a2\u3057\u306a\u3089 <a href=\"https:\/\/steelprogroup.com\/ja\/tool-steel\/h13\/\">H13\u5de5\u5177\u92fc\u677f\u307e\u305f\u306f\u68d2<\/a> \u6b21\u306e\u30d7\u30ed\u30b8\u30a7\u30af\u30c8\u3067\u306f\u3001SteelPro Group \u304c\u304a\u624b\u4f1d\u3044\u3057\u307e\u3059\u3002\u30ab\u30b9\u30bf\u30e0\u5f62\u72b6\u3001\u7cbe\u5bc6\u6a5f\u68b0\u52a0\u5de5\u3001\u9ad8\u6e29\u30a2\u30d7\u30ea\u30b1\u30fc\u30b7\u30e7\u30f3\u5411\u3051\u306e\u30ab\u30b9\u30bf\u30de\u30a4\u30ba\u3055\u308c\u305f\u30bd\u30ea\u30e5\u30fc\u30b7\u30e7\u30f3\u306a\u3069\u3001\u304a\u5ba2\u69d8\u306e\u30cb\u30fc\u30ba\u3092\u6e80\u305f\u3059\u4fe1\u983c\u6027\u306e\u9ad8\u3044\u6700\u9ad8\u54c1\u8cea\u306e\u88fd\u54c1\u3092\u63d0\u4f9b\u3057\u307e\u3059\u3002<\/p><p class=\"wp-block-paragraph\"><\/p>","protected":false},"excerpt":{"rendered":"<p>SteelPro Group \u3067\u306f\u3001\u30d0\u30fc\u3001\u30ed\u30c3\u30c9\u3001\u30ab\u30b9\u30bf\u30e0\u5f62\u72b6\u306a\u3069\u3001\u3055\u307e\u3056\u307e\u306a\u5f62\u72b6\u306e H13 \u5de5\u5177\u92fc\u3092\u4f9b\u7d66\u3057\u3066\u3044\u307e\u3059\u3002\u5f53\u793e\u306e H13 \u92fc [\u2026]<\/p>","protected":false},"author":12,"featured_media":19992,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_acf_changed":false,"_eb_attr":"","rank_math_lock_modified_date":false,"site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"var(--ast-global-color-4)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"categories":[4297,4294,4296,4293],"tags":[],"class_list":["post-20020","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-property-h13","category-grades-tool-steel","category-h13","category-tool-steel"],"acf":[],"_links":{"self":[{"href":"https:\/\/steelprogroup.com\/ja\/wp-json\/wp\/v2\/posts\/20020","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/steelprogroup.com\/ja\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/steelprogroup.com\/ja\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/steelprogroup.com\/ja\/wp-json\/wp\/v2\/users\/12"}],"replies":[{"embeddable":true,"href":"https:\/\/steelprogroup.com\/ja\/wp-json\/wp\/v2\/comments?post=20020"}],"version-history":[{"count":0,"href":"https:\/\/steelprogroup.com\/ja\/wp-json\/wp\/v2\/posts\/20020\/revisions"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/steelprogroup.com\/ja\/wp-json\/wp\/v2\/media\/19992"}],"wp:attachment":[{"href":"https:\/\/steelprogroup.com\/ja\/wp-json\/wp\/v2\/media?parent=20020"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/steelprogroup.com\/ja\/wp-json\/wp\/v2\/categories?post=20020"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/steelprogroup.com\/ja\/wp-json\/wp\/v2\/tags?post=20020"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}