{"id":20139,"date":"2024-12-30T09:40:00","date_gmt":"2024-12-30T01:40:00","guid":{"rendered":"https:\/\/steelprogroup.com\/?p=20139"},"modified":"2025-01-14T11:49:48","modified_gmt":"2025-01-14T03:49:48","slug":"p20","status":"publish","type":"post","link":"https:\/\/steelprogroup.com\/ja\/tool-steel\/grades\/p20\/","title":{"rendered":"\u5de5\u5177\u92fc AISI P20 \u91d1\u578b\u92fc | 3Cr2Mo | 1.2311"},"content":{"rendered":"<p class=\"wp-block-paragraph\">SteelPro Group \u306f\u3001\u9ad8\u54c1\u8cea\u306e P20 \u5de5\u5177\u92fc\u306e\u4fe1\u983c\u3067\u304d\u308b\u30b5\u30d7\u30e9\u30a4\u30e4\u30fc\u3067\u3059\u3002\u5f53\u793e\u306e P20 \u88fd\u54c1\u306f\u3001\u305d\u306e\u5f37\u976d\u6027\u3068\u6a5f\u68b0\u52a0\u5de5\u6027\u3067\u77e5\u3089\u308c\u3066\u304a\u308a\u3001\u91d1\u578b\u88fd\u4f5c\u3084\u5de5\u5177\u88fd\u4f5c\u306b\u6700\u9069\u3067\u3059\u3002\u6b63\u78ba\u306a\u8a31\u5bb9\u5dee\u3068\u30ab\u30b9\u30bf\u30e0 \u30b5\u30a4\u30ba\u304c\u5229\u7528\u53ef\u80fd\u3067\u3001\u304a\u5ba2\u69d8\u306e\u92fc\u6750\u30cb\u30fc\u30ba\u3092\u6e80\u305f\u3059\u4fe1\u983c\u6027\u306e\u9ad8\u3044\u30bd\u30ea\u30e5\u30fc\u30b7\u30e7\u30f3\u3092\u63d0\u4f9b\u3057\u307e\u3059\u3002<\/p><h2 class=\"wp-block-heading\">P20 \u5de5\u5177\u92fc\u3068\u306f\u4f55\u3067\u3059\u304b?<\/h2><p class=\"wp-block-paragraph\">P20 \u5de5\u5177\u92fc\u306f\u3001\u4e2d\u7a0b\u5ea6\u306e\u5f37\u5ea6\u30ec\u30d9\u30eb\u3067\u512a\u308c\u305f\u8010\u4e45\u6027\u3092\u767a\u63ee\u3059\u308b\u67d4\u8edf\u6027\u306e\u3042\u308b\u4f4e\u5408\u91d1\u91d1\u5c5e\u3067\u3059\u3002\u30af\u30ed\u30e0\u3068\u30cb\u30c3\u30b1\u30eb\u306e\u542b\u6709\u91cf\u306b\u3088\u308a\u3001\u976d\u6027\u3068\u786c\u5ea6\u304c\u5411\u4e0a\u3057\u307e\u3059\u3002P20 \u306f\u3001\u512a\u308c\u305f\u52a0\u5de5\u6027\u3068\u7814\u78e8\u6027\u3082\u5099\u3048\u3066\u3044\u307e\u3059\u3002&nbsp;<\/p><p class=\"wp-block-paragraph\">SteelPro Group P20 \u92fc\u306f\u3001\u5c04\u51fa\u6210\u5f62\u91d1\u578b\u306e\u30ad\u30e3\u30d3\u30c6\u30a3\u3001\u30c4\u30fc\u30eb\u3001\u4e9c\u925b\u30c0\u30a4\u30ab\u30b9\u30c8\u91d1\u578b\u306b\u3088\u304f\u4f7f\u7528\u3055\u308c\u3001\u901a\u5e38\u306f 300 HBW \u524d\u5f8c\u3067\u30d7\u30ea\u30cf\u30fc\u30c9\u30f3\u51e6\u7406\u3055\u308c\u305f\u72b6\u614b\u3067\u4f9b\u7d66\u3055\u308c\u307e\u3059\u3002\u3053\u306e\u92fc\u306f\u3001\u7a92\u5316\u3084\u6d78\u70ad\u306a\u3069\u306e\u8ffd\u52a0\u51e6\u7406\u3092\u65bd\u3059\u3053\u3068\u3067\u7279\u6027\u3092\u5411\u4e0a\u3055\u305b\u308b\u3053\u3068\u304c\u3067\u304d\u307e\u3059\u3002<\/p><h2 class=\"wp-block-heading\">P20 \u92fc\u306b\u76f8\u5f53\u3059\u308b\u3082\u306e\u306f\u4f55\u3067\u3059\u304b?<\/h2><p class=\"wp-block-paragraph\">L2 \u92fc\u306f\u3001\u4e2d\u56fd GB\/T 1299 \u898f\u683c\u306e 3Cr2Mo\u3001ASTM A681 \u898f\u683c\u306e P20\u3001DIN EN ISO 4957 \u898f\u683c\u306e 1.2311 \u306b\u76f8\u5f53\u3057\u307e\u3059\u3002<\/p><h2 class=\"wp-block-heading\">P20\u5de5\u5177\u92fc\u306e\u4e3b\u306a\u7279\u6027<\/h2><ul class=\"wp-block-list\"><li><strong>\u9ad8\u3044\u976d\u6027<\/strong>: \u5272\u308c\u3084\u885d\u6483\u306b\u5bfe\u3059\u308b\u8010\u6027\u304c\u512a\u308c\u3066\u304a\u308a\u3001\u30b9\u30c8\u30ec\u30b9\u4e0b\u3067\u3082\u8010\u4e45\u6027\u3092\u78ba\u4fdd\u3057\u307e\u3059\u3002<\/li>\n\n<li><strong>\u512a\u308c\u305f\u52a0\u5de5\u6027<\/strong>: \u6a5f\u68b0\u52a0\u5de5\u304c\u5bb9\u6613\u3067\u3001\u8907\u96d1\u306a\u90e8\u54c1\u3092\u52b9\u7387\u7684\u306b\u52a0\u5de5\u3067\u304d\u307e\u3059\u3002<\/li>\n\n<li><strong>\u30d7\u30ec\u30cf\u30fc\u30c9\u30f3<\/strong>: 300 HBW \u3067\u7d0d\u54c1\u3057\u3001\u3055\u3089\u306a\u308b\u71b1\u51e6\u7406\u306e\u5fc5\u8981\u6027\u3092\u6700\u5c0f\u9650\u306b\u6291\u3048\u307e\u3057\u305f\u3002<\/li>\n\n<li><strong>\u4e2d\u7a0b\u5ea6\u306e\u8010\u6469\u8017\u6027<\/strong>: \u904e\u5ea6\u306a\u786c\u5ea6\u304c\u306a\u304f\u3001\u512a\u308c\u305f\u8010\u6469\u8017\u6027\u3092\u767a\u63ee\u3057\u307e\u3059\u3002<\/li>\n\n<li><strong>\u5bf8\u6cd5\u5b89\u5b9a\u6027<\/strong>: \u6a5f\u68b0\u52a0\u5de5\u3084\u71b1\u51e6\u7406\u5de5\u7a0b\u3067\u3082\u5f62\u72b6\u3068\u30b5\u30a4\u30ba\u3092\u7dad\u6301\u3057\u307e\u3059\u3002<\/li><\/ul><h2 class=\"wp-block-heading\">P20 \u5de5\u5177\u92fc\u88fd\u54c1\u306e\u5f62\u72b6\u3068\u4f9b\u7d66\u7bc4\u56f2<\/h2><p class=\"wp-block-paragraph\">SteelPro Group \u306f\u3001\u4e16\u754c\u6a19\u6e96\u306b\u6e96\u62e0\u3057\u305f\u9ad8\u54c1\u8cea\u306e P20 \u5de5\u5177\u92fc\u6750\u6599\u3092\u63d0\u4f9b\u3057\u3066\u3044\u307e\u3059\u3002\u53b3\u683c\u306a\u8a31\u5bb9\u5dee\u7ba1\u7406\u306b\u3088\u308a\u3001\u4fe1\u983c\u6027\u304c\u9ad8\u304f\u7cbe\u5bc6\u306a\u6750\u6599\u3092\u4fdd\u8a3c\u3057\u307e\u3059\u3002\u307e\u305f\u3001\u304a\u5ba2\u69d8\u306e\u72ec\u81ea\u306e\u8981\u4ef6\u3092\u6e80\u305f\u3059\u30ab\u30b9\u30bf\u30de\u30a4\u30ba\u3055\u308c\u305f\u30b5\u30a4\u30ba\u3082\u63d0\u4f9b\u3057\u3066\u3044\u307e\u3059\u3002<\/p><figure class=\"wp-block-table\"><table><tbody><tr><td><strong>\u88fd\u54c1\u5f62\u614b<\/strong><\/td><td><strong>\u30b5\u30a4\u30ba\u7bc4\u56f2\uff08\u30e1\u30fc\u30c8\u30eb\u6cd5\uff09<\/strong><\/td><td><strong>\u30b5\u30a4\u30ba\u7bc4\u56f2\uff08\u30e4\u30fc\u30c9\u30dd\u30f3\u30c9\u6cd5\uff09<\/strong><\/td><\/tr><tr><td>\u5de5\u5177\u92fc\u677f<\/td><td>\u539a\u3055: 10 mm \uff5e 300 mm\u5e45: 100 mm \uff5e 2500 mm\u9577\u3055: 200 mm \uff5e 6000 mm<\/td><td>\u539a\u3055: 0.4 \u30a4\u30f3\u30c1\uff5e 12 \u30a4\u30f3\u30c1\u5e45: 4 \u30a4\u30f3\u30c1\uff5e 100 \u30a4\u30f3\u30c1\u9577\u3055: 8 \u30a4\u30f3\u30c1\uff5e 236 \u30a4\u30f3\u30c1<\/td><\/tr><tr><td>\u5de5\u5177\u92fc\u30d0\u30fc<\/td><td>\u4e38\u68d2: \u76f4\u5f84 20 mm \uff5e 500 mm \u89d2\u68d2: \u8fba\u306e\u9577\u3055 20 mm \uff5e 300 mm \u9577\u3055: 3000 mm \uff5e 6000 mm<\/td><td>\u4e38\u68d2: \u76f4\u5f84 0.8 \u30a4\u30f3\u30c1\u304b\u3089 20 \u30a4\u30f3\u30c1\u89d2\u68d2: \u8fba\u306e\u9577\u3055 0.8 \u30a4\u30f3\u30c1\u304b\u3089 12 \u30a4\u30f3\u30c1\u9577\u3055: 118 \u30a4\u30f3\u30c1\u304b\u3089 236 \u30a4\u30f3\u30c1<\/td><\/tr><tr><td>\u5de5\u5177\u92fc\u30d6\u30ed\u30c3\u30af<\/td><td>\u5e45\/\u9577\u3055: 100 mm\uff5e1200 mm\u9ad8\u3055\/\u539a\u3055: 50 mm\uff5e400 mm<\/td><td>\u5e45\/\u9577\u3055: 4\u30a4\u30f3\u30c1\uff5e47\u30a4\u30f3\u30c1\u9ad8\u3055\/\u539a\u3055: 2\u30a4\u30f3\u30c1\uff5e16\u30a4\u30f3\u30c1<\/td><\/tr><tr><td>\u5de5\u5177\u92fc\u935b\u9020\u54c1<\/td><td>\u8981\u4ef6\u306b\u5fdc\u3058\u3066\u30ab\u30b9\u30bf\u30de\u30a4\u30ba\u3055\u308c\u305f\u30b5\u30a4\u30ba<\/td><td>\u8981\u4ef6\u306b\u5fdc\u3058\u3066\u30ab\u30b9\u30bf\u30de\u30a4\u30ba\u3055\u308c\u305f\u30b5\u30a4\u30ba<\/td><\/tr><\/tbody><\/table><\/figure><h2 class=\"wp-block-heading\">P20\u5de5\u5177\u92fc\u306e\u5316\u5b66\u7d44\u6210<\/h2><figure class=\"wp-block-table\"><table><tbody><tr><td><strong>\u30a8\u30ec\u30e1\u30f3\u30c8<\/strong><\/td><td><strong>\u69cb\u6210\uff08%\uff09<\/strong><\/td><\/tr><tr><td>\u30ab\u30fc\u30dc\u30f3\uff08C\uff09<\/td><td>0.28 &#8211; 0.40<\/td><\/tr><tr><td>\u30af\u30ed\u30e0\uff08Cr\uff09<\/td><td>1.4 &#8211; 2.0<\/td><\/tr><tr><td>\u9244\uff08Fe\uff09<\/td><td>97\u3001\u30d0\u30e9\u30f3\u30b9\u3068\u3057\u3066<\/td><\/tr><tr><td>\u30de\u30f3\u30ac\u30f3 (Mn)<\/td><td>0.60 &#8211; 1.0<\/td><\/tr><tr><td>\u30e2\u30ea\u30d6\u30c7\u30f3 (Mo)<\/td><td>0.30 &#8211; 0.55<\/td><\/tr><tr><td>\u30ea\u30f3 (P)<\/td><td>\u2264 0.030<\/td><\/tr><tr><td>\u30b1\u30a4\u7d20 (Si)<\/td><td>0.20 &#8211; 0.80<\/td><\/tr><tr><td>\u786b\u9ec4\uff08S\uff09<\/td><td>\u2264 0.030<\/td><\/tr><\/tbody><\/table><\/figure><h2 class=\"wp-block-heading\">P20\u5de5\u5177\u92fc\u306e\u7269\u7406\u7684\u7279\u6027<\/h2><figure class=\"wp-block-table\"><table><tbody><tr><td><strong>\u30d7\u30ed\u30d1\u30c6\u30a3<\/strong><\/td><td><strong>\u30e1\u30c8\u30ea\u30c3\u30af\u5024<\/strong><\/td><td><strong>\u30a4\u30f3\u30da\u30ea\u30a2\u30eb\u30fb\u30d0\u30ea\u30e5\u30fc<\/strong><\/td><\/tr><tr><td>\u5bc6\u5ea6<\/td><td>7.85 g\/cc<\/td><td>0.284 lb\/in\u00b3<\/td><\/tr><tr><td>\u71b1\u81a8\u5f35\u4fc2\u6570<\/td><td>12.8 \u00b5m\/m\u00b7\u00b0C (20.0\u00b0C\u6642)<\/td><td>7.10 \u00b5in\/in\u00b7\u00b0F (68.0\u00b0F \u306e\u3068\u304d)<\/td><\/tr><tr><td>\u71b1\u4f1d\u5c0e\u7387<\/td><td>29.0 \u2013 34.0 W\/m\u00b7K<\/td><td>201 \u2013 236 BTU\u00b7in\/hr\u00b7ft\u00b2\u00b7\u00b0F<\/td><\/tr><tr><td>\u6bd4\u71b1<\/td><td>460 J\/kg-K<\/td><td>0.110 BTU\/lb-\u00b0F<\/td><\/tr><\/tbody><\/table><\/figure><h2 class=\"wp-block-heading\">P20\u5de5\u5177\u92fc\u306e\u6a5f\u68b0\u7684\u6027\u8cea<\/h2><figure class=\"wp-block-table\"><table><tbody><tr><td><strong>\u30d7\u30ed\u30d1\u30c6\u30a3<\/strong><\/td><td><strong>\u30e1\u30c8\u30ea\u30c3\u30af\u5024<\/strong><\/td><td><strong>\u30a4\u30f3\u30da\u30ea\u30a2\u30eb\u30fb\u30d0\u30ea\u30e5\u30fc<\/strong><\/td><\/tr><tr><td>\u786c\u5ea6\u3001\u30d6\u30ea\u30cd\u30eb<\/td><td>300<\/td><td>300<\/td><\/tr><tr><td>\u786c\u5ea6\u3001\u30ed\u30c3\u30af\u30a6\u30a7\u30ebC<\/td><td>30<\/td><td>30<\/td><\/tr><tr><td>\u5f15\u5f35\u5f37\u3055\u3001\u6975\u9650<\/td><td>965 \u2013 1030 MPa<\/td><td>140000 \u2013 150000 psi<\/td><\/tr><tr><td>\u5f15\u5f35\u5f37\u5ea6\u3001\u964d\u4f0f\u5f37\u5ea6<\/td><td>827 \u2013 862 MPa<\/td><td>120000 \u2013 125000 psi<\/td><\/tr><tr><td>\u7834\u65ad\u6642\u306e\u4f38\u3073\uff0850 mm \/ 2\u30a4\u30f3\u30c1\uff09<\/td><td>20 %<\/td><td>20 %<\/td><\/tr><tr><td>\u5f3e\u6027\u4fc2\u6570<\/td><td>205GPa<\/td><td>29700 ksi<\/td><\/tr><tr><td>\u5727\u7e2e\u5f37\u5ea6<\/td><td>862MPa<\/td><td>125000 psi<\/td><\/tr><tr><td>\u30b7\u30e3\u30eb\u30d4\u30fc\u885d\u6483\u8a66\u9a13\uff08V\u30ce\u30c3\u30c1\uff09<\/td><td>27.1 \u2013 33.9 \u30b8\u30e5\u30fc\u30eb<\/td><td>20.0 \u2013 25.0 \u30d5\u30a3\u30fc\u30c8\u30dd\u30f3\u30c9<\/td><\/tr><\/tbody><\/table><\/figure><h2 class=\"wp-block-heading\">P20\u5de5\u5177\u92fc\u71b1\u51e6\u7406<\/h2><p class=\"wp-block-paragraph\">\u5f53\u793e\u3067\u306f\u3001\u512a\u308c\u305f\u6a5f\u68b0\u52a0\u5de5\u6027\u3068\u6700\u5c0f\u9650\u306e\u6b8b\u7559\u5fdc\u529b\u3092\u4fdd\u8a3c\u3059\u308b\u713c\u304d\u306a\u307e\u3057\u72b6\u614b\u306e P20 \u5de5\u5177\u92fc\u3092\u63d0\u4f9b\u3057\u3066\u3044\u307e\u3059\u3002\u3053\u306e\u305f\u3081\u3001\u5f53\u793e\u306e P20 \u306f\u91d1\u578b\u88fd\u4f5c\u3084\u5de5\u5177\u88fd\u4f5c\u306e\u7528\u9014\u306b\u6700\u9069\u3067\u3042\u308a\u3001\u3042\u3089\u3086\u308b\u30d7\u30ed\u30b8\u30a7\u30af\u30c8\u3067\u4fe1\u983c\u6027\u306e\u9ad8\u3044\u6027\u80fd\u3068\u7cbe\u5ea6\u3092\u5b9f\u73fe\u3057\u307e\u3059\u3002<\/p><h3 class=\"wp-block-heading\">\u935b\u9020<\/h3><p class=\"wp-block-paragraph\">P20 \u5de5\u5177\u92fc\u306e\u5834\u5408\u3001\u7406\u60f3\u7684\u306a\u935b\u9020\u6e29\u5ea6\u7bc4\u56f2\u306f 1149\u00b0C (2100\u00b0F) \uff5e 1260\u00b0C (2300\u00b0F) \u3067\u3059\u3002\u935b\u9020\u5f8c\u306f\u3001\u92fc\u304c\u5272\u308c\u308b\u306e\u3092\u9632\u3050\u305f\u3081\u3001\u3086\u3063\u304f\u308a\u3068\u51b7\u5374\u3057\u3066\u304f\u3060\u3055\u3044\u3002<\/p><h3 class=\"wp-block-heading\">\u30a2\u30cb\u30fc\u30ea\u30f3\u30b0<\/h3><p class=\"wp-block-paragraph\">P20 \u3092\u713c\u304d\u306a\u307e\u3059\u306b\u306f\u3001\u92fc\u3092 760 \uff5e 788\u00b0C (1400 \uff5e 1450\u00b0F) \u306e\u6e29\u5ea6\u7bc4\u56f2\u306b\u52a0\u71b1\u3057\u307e\u3059\u3002\u539a\u3055 25.4mm (1 \u30a4\u30f3\u30c1) \u3054\u3068\u306b 1 \u6642\u9593\u3001\u6700\u4f4e 2 \u6642\u9593\u3001\u6e29\u5ea6\u3092\u7dad\u6301\u3057\u307e\u3059\u3002\u4fdd\u6301\u5f8c\u3001\u92fc\u3092\u7089\u5185\u3067 1 \u6642\u9593\u3042\u305f\u308a 4\u00b0C (40\u00b0F) \u3092\u8d85\u3048\u306a\u3044\u901f\u5ea6\u3067\u5f90\u3005\u306b\u51b7\u5374\u3057\u3001\u5ba4\u6e29\u306b\u5230\u9054\u3055\u305b\u307e\u3059\u3002<\/p><h3 class=\"wp-block-heading\">\u30b9\u30c8\u30ec\u30b9\u89e3\u6d88<\/h3><p class=\"wp-block-paragraph\">\u6a5f\u68b0\u52a0\u5de5\u5f8c\u307e\u305f\u306f\u65ad\u7d9a\u7684\u306a\u4f7f\u7528\u4e2d\u306b\u3001P20 \u3092 482\u00b0C (900\u00b0F) \u306b\u52a0\u71b1\u3057\u307e\u3059\u3002\u539a\u3055 25.4mm (1 \u30a4\u30f3\u30c1) \u3054\u3068\u306b 1 \u6642\u9593\u6e29\u5ea6\u3092\u7dad\u6301\u3057\u3001\u305d\u306e\u5f8c\u6750\u6599\u3092\u5ba4\u6e29\u307e\u3067\u7a7a\u6c17\u4e2d\u3067\u51b7\u5374\u3057\u307e\u3059\u3002\u3053\u306e\u624b\u9806\u306b\u3088\u308a\u3001\u5185\u90e8\u5fdc\u529b\u304c\u7de9\u548c\u3055\u308c\u3001\u5bf8\u6cd5\u306e\u9762\u3067\u92fc\u306e\u5b89\u5b9a\u6027\u304c\u5411\u4e0a\u3057\u307e\u3059\u3002<\/p><h3 class=\"wp-block-heading\">\u786c\u5316<\/h3><ul class=\"wp-block-list\"><li><strong>\u4e88\u71b1<\/strong>: P20 \u3092 1 \u6642\u9593\u3042\u305f\u308a 222\u00b0C (400\u00b0F) \u3092\u8d85\u3048\u306a\u3044\u901f\u5ea6\u3067 621 \uff5e 677\u00b0C (1150 \uff5e 1250\u00b0F) \u306e\u6e29\u5ea6\u307e\u3067\u52a0\u71b1\u3057\u307e\u3059\u3002\u3053\u306e\u6e29\u5ea6\u3067\u92fc\u304c\u5747\u4e00\u306b\u306a\u308b\u307e\u3067\u5f85\u3061\u307e\u3059\u3002<\/li>\n\n<li><strong>\u30aa\u30fc\u30b9\u30c6\u30ca\u30a4\u30c8\u5316<\/strong>: \u4e88\u71b1\u5f8c\u3001\u92fc\u3092\u6025\u901f\u306b 843\u00b0C (1550\u00b0F) \u307e\u3067\u52a0\u71b1\u3057\u307e\u3059\u3002\u6700\u521d\u306e 25.4mm (1 \u30a4\u30f3\u30c1) \u306e\u539a\u3055\u3092 30 \u5206\u9593\u6d78\u3057\u3001\u305d\u306e\u5f8c 1 \u30a4\u30f3\u30c1\u3054\u3068\u306b\u3055\u3089\u306b 15 \u5206\u9593\u6d78\u3057\u307e\u3059\u3002<\/li>\n\n<li><strong>\u713c\u304d\u5165\u308c<\/strong>: \u52a0\u5727\u30ac\u30b9\u307e\u305f\u306f\u4e2d\u65ad\u6cb9\u713c\u5165\u308c\u3092\u4f7f\u7528\u3057\u3066\u3001\u92fc\u3092 66 \uff5e 51\u00b0C (150 \uff5e 125\u00b0F) \u307e\u3067\u51b7\u5374\u3057\u307e\u3059\u3002\u6cb9\u713c\u5165\u308c\u306e\u5834\u5408\u306f\u3001\u92fc\u304c\u7d04 482\u00b0C (900\u00b0F) \u3067\u9ed2\u304f\u306a\u308b\u307e\u3067\u713c\u5165\u308c\u3057\u3001\u305d\u306e\u5f8c\u3001\u9759\u6b62\u7a7a\u6c17\u4e2d\u3067\u51b7\u5374\u3092\u5b8c\u4e86\u3057\u307e\u3059\u3002<\/li><\/ul><h3 class=\"wp-block-heading\">\u713c\u304d\u623b\u3057<\/h3><p class=\"wp-block-paragraph\">\u713c\u304d\u5165\u308c\u5f8c\u3001\u76f4\u3061\u306b\u713c\u304d\u623b\u3057\u3092\u884c\u3046\u5fc5\u8981\u304c\u3042\u308a\u307e\u3059\u3002P20 \u3092 482 \uff5e 593\u00b0C (900 \uff5e 1100\u00b0F) \u306e\u6e29\u5ea6\u7bc4\u56f2\u3067\u3001\u539a\u3055 25.4 mm (1 \u30a4\u30f3\u30c1) \u3042\u305f\u308a 1 \u6642\u9593\u52a0\u71b1\u3057\u3001\u6700\u4f4e 2 \u6642\u9593\u4fdd\u6301\u3057\u307e\u3059\u3002\u713c\u304d\u623b\u3057\u5f8c\u3001\u92fc\u3092\u7a7a\u6c17\u4e2d\u3067\u5ba4\u6e29\u307e\u3067\u51b7\u5374\u3057\u307e\u3059\u3002<\/p><h2 class=\"wp-block-heading\">P20\u5de5\u5177\u92fc\u306e\u7528\u9014<\/h2><p class=\"wp-block-paragraph\">P20 \u5de5\u5177\u92fc\u306f\u4e3b\u306b\u4ee5\u4e0b\u306e\u7528\u9014\u306b\u4f7f\u7528\u3055\u308c\u307e\u3059\u3002<\/p><ul class=\"wp-block-list\"><li>\u5c04\u51fa\u6210\u5f62\u91d1\u578b<\/li>\n\n<li>\u30d6\u30ed\u30fc\u6210\u5f62\u30c4\u30fc\u30eb<\/li>\n\n<li>\u5727\u7e2e\u91d1\u578b<\/li>\n\n<li>\u30c0\u30a4\u30ab\u30b9\u30c8\u91d1\u578b<\/li>\n\n<li>\u6210\u5f62\u91d1\u578b<\/li>\n\n<li>\u30b3\u30a2\u30d4\u30f3\u3068\u30a4\u30f3\u30b5\u30fc\u30c8<\/li><\/ul><h2 class=\"wp-block-heading\">4140 \u30b9\u30c1\u30fc\u30eb vs P20 \u30b9\u30c1\u30fc\u30eb<\/h2><p class=\"wp-block-paragraph\">4140 \u306f\u9ad8\u5fdc\u529b\u306e\u7528\u9014\u306b\u4f7f\u7528\u3055\u308c\u307e\u3059\u304c\u3001P20 \u306f\u4e2d\u7a0b\u5ea6\u306e\u5f37\u5ea6\u304c\u6c42\u3081\u3089\u308c\u308b\u30c4\u30fc\u30eb\u306b\u9069\u3057\u3066\u3044\u307e\u3059\u3002<\/p><p class=\"wp-block-paragraph\">4140 \u92fc\u306f\u3001\u30af\u30ed\u30e0\u3068\u30e2\u30ea\u30d6\u30c7\u30f3\u306e\u542b\u6709\u91cf\u306b\u3088\u308a\u5f37\u5ea6\u3068\u786c\u5ea6\u304c\u9ad8\u304f\u3001\u30ae\u30a2\u3084\u30b7\u30e3\u30d5\u30c8\u306a\u3069\u306e\u9ad8\u8ca0\u8377\u7528\u9014\u306b\u9069\u3057\u3066\u3044\u307e\u3059\u3002\u30d7\u30ea\u30cf\u30fc\u30c9\u30f3\u5de5\u5177\u92fc\u306e P20 \u306f\u91d1\u578b\u88fd\u9020\u306b\u6700\u9069\u3067\u3001\u30d7\u30e9\u30b9\u30c1\u30c3\u30af\u5c04\u51fa\u6210\u5f62\u91d1\u578b\u3084\u30c0\u30a4\u30ab\u30b9\u30c8\u306b\u512a\u308c\u305f\u52a0\u5de5\u6027\u3068\u976d\u6027\u3092\u63d0\u4f9b\u3057\u307e\u3059\u3002&nbsp;<\/p><h2 class=\"wp-block-heading\">P20\u92fc\u3068A2\u92fc\u306e\u6bd4\u8f03<\/h2><p class=\"wp-block-paragraph\">P20\u306f\u30d7\u30e9\u30b9\u30c1\u30c3\u30af\u6210\u5f62\u306b\u9069\u3057\u3066\u3044\u307e\u3059\u304c\u3001 <a href=\"https:\/\/steelprogroup.com\/ja\/tool-steel\/grades\/a2\/\">A2\u5de5\u5177\u92fc<\/a> \u9ad8\u7cbe\u5ea6\u3001\u9ad8\u8010\u6469\u8017\u5de5\u5177\u306b\u512a\u308c\u3066\u3044\u307e\u3059\u3002<\/p><p class=\"wp-block-paragraph\">P20 \u92fc\u306f\u30d7\u30ec\u30cf\u30fc\u30c9\u30f3\u92fc\u3067\u3001\u4e3b\u306b\u91d1\u578b\u88fd\u9020\u306b\u4f7f\u7528\u3055\u308c\u3001\u512a\u308c\u305f\u52a0\u5de5\u6027\u3068\u976d\u6027\u3092\u5099\u3048\u3066\u3044\u307e\u3059\u3002A2 \u92fc\u306f\u70ad\u7d20\u542b\u6709\u91cf\u304c\u9ad8\u304f\u3001\u976d\u6027\u3068\u8010\u6469\u8017\u6027\u306b\u512a\u308c\u3066\u3044\u308b\u305f\u3081\u3001\u5207\u524a\u5de5\u5177\u3001\u30c0\u30a4\u3001\u30d1\u30f3\u30c1\u306b\u9069\u3057\u3066\u3044\u307e\u3059\u3002&nbsp;<\/p><h2 class=\"wp-block-heading\">H13\u92fc\u3068P20\u92fc<\/h2><p class=\"wp-block-paragraph\"><a href=\"https:\/\/steelprogroup.com\/ja\/tool-steel\/h13\/\">H13\u92fc\u677f<\/a> \u306f\u9ad8\u6e29\u7528\u9014\u306b\u9069\u3057\u3066\u304a\u308a\u3001P20 \u306f\u4e2d\u5f37\u5ea6\u306e\u5de5\u5177\u306b\u6700\u9069\u3067\u3059\u3002<\/p><p class=\"wp-block-paragraph\">H13 \u306f\u3001\u9ad8\u6e29\u3067\u306e\u71b1\u306b\u3088\u308b\u5272\u308c\u3084\u6469\u8017\u306b\u5bfe\u3059\u308b\u5f37\u3044\u8010\u6027\u3067\u77e5\u3089\u308c\u308b\u8010\u71b1\u5de5\u5177\u92fc\u3067\u3001\u30c0\u30a4\u30ab\u30b9\u30c8\u3084\u71b1\u9593\u935b\u9020\u5de5\u5177\u306b\u6700\u9069\u3067\u3059\u3002\u4e00\u65b9\u3001P20 \u306f\u30d7\u30e9\u30b9\u30c1\u30c3\u30af\u91d1\u578b\u306a\u3069\u306e\u51b7\u9593\u52a0\u5de5\u5de5\u5177\u306b\u4f7f\u7528\u3055\u308c\u3001\u6a5f\u68b0\u52a0\u5de5\u6027\u3068\u5bf8\u6cd5\u5b89\u5b9a\u6027\u304c\u9ad8\u304f\u8a55\u4fa1\u3055\u308c\u3066\u3044\u307e\u3059\u3002&nbsp;<\/p><h2 class=\"wp-block-heading\">\u304a\u5ba2\u69d8\u306e\u30cb\u30fc\u30ba\u306b\u5408\u308f\u305b\u305f\u30ab\u30b9\u30bf\u30e0P20\u5de5\u5177\u92fc\u30bd\u30ea\u30e5\u30fc\u30b7\u30e7\u30f3<\/h2><p class=\"wp-block-paragraph\">\u4fe1\u983c\u6027\u306e\u9ad8\u3044 P20 \u5de5\u5177\u92fc\u3092\u304a\u63a2\u3057\u306a\u3089\u3001SteelPro Group \u306b\u304a\u4efb\u305b\u304f\u3060\u3055\u3044\u3002\u30d7\u30ec\u30fc\u30c8\u3084\u30d0\u30fc\u306a\u3069\u3001\u3055\u307e\u3056\u307e\u306a\u88fd\u54c1\u3092\u53d6\u308a\u63c3\u3048\u3066\u304a\u308a\u3001\u304a\u5ba2\u69d8\u306e\u4ed5\u69d8\u306b\u5408\u308f\u305b\u305f\u30ab\u30b9\u30bf\u30e0 \u30b5\u30a4\u30ba\u3082\u3054\u7528\u610f\u3057\u3066\u3044\u307e\u3059\u3002\u5f53\u793e\u306e\u30b5\u30fc\u30d3\u30b9\u306b\u306f\u3001\u5207\u65ad\u3001\u7814\u78e8\u3001\u305d\u306e\u4ed6\u306e\u6a5f\u68b0\u52a0\u5de5\u30aa\u30d7\u30b7\u30e7\u30f3\u304c\u542b\u307e\u308c\u3066\u304a\u308a\u3001\u304a\u5ba2\u69d8\u306e\u30d7\u30ed\u30b8\u30a7\u30af\u30c8\u306b\u6700\u9069\u306a\u30bd\u30ea\u30e5\u30fc\u30b7\u30e7\u30f3\u3092\u63d0\u4f9b\u3057\u307e\u3059\u3002&nbsp;<\/p>","protected":false},"excerpt":{"rendered":"<p>SteelPro Group \u306f\u3001\u9ad8\u54c1\u8cea\u306e P20 \u5de5\u5177\u92fc\u306e\u4fe1\u983c\u3067\u304d\u308b\u30b5\u30d7\u30e9\u30a4\u30e4\u30fc\u3067\u3059\u3002\u305d\u306e\u5f37\u976d\u6027\u3068\u6a5f\u68b0\u52a0\u5de5\u6027\u3067\u77e5\u3089\u308c\u308b\u5f53\u793e\u306e [\u2026]<\/p>","protected":false},"author":12,"featured_media":20128,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_acf_changed":false,"_eb_attr":"","rank_math_lock_modified_date":false,"site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"var(--ast-global-color-4)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"categories":[4294,4293],"tags":[],"class_list":["post-20139","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-grades-tool-steel","category-tool-steel"],"acf":[],"_links":{"self":[{"href":"https:\/\/steelprogroup.com\/ja\/wp-json\/wp\/v2\/posts\/20139","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/steelprogroup.com\/ja\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/steelprogroup.com\/ja\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/steelprogroup.com\/ja\/wp-json\/wp\/v2\/users\/12"}],"replies":[{"embeddable":true,"href":"https:\/\/steelprogroup.com\/ja\/wp-json\/wp\/v2\/comments?post=20139"}],"version-history":[{"count":0,"href":"https:\/\/steelprogroup.com\/ja\/wp-json\/wp\/v2\/posts\/20139\/revisions"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/steelprogroup.com\/ja\/wp-json\/wp\/v2\/media\/20128"}],"wp:attachment":[{"href":"https:\/\/steelprogroup.com\/ja\/wp-json\/wp\/v2\/media?parent=20139"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/steelprogroup.com\/ja\/wp-json\/wp\/v2\/categories?post=20139"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/steelprogroup.com\/ja\/wp-json\/wp\/v2\/tags?post=20139"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}