{"id":21410,"date":"2025-03-16T06:01:00","date_gmt":"2025-03-15T22:01:00","guid":{"rendered":"https:\/\/steelprogroup.com\/?p=21410"},"modified":"2025-03-17T10:18:14","modified_gmt":"2025-03-17T02:18:14","slug":"maraging-steel-guide","status":"publish","type":"post","link":"https:\/\/steelprogroup.com\/ru\/alloy-steel\/maraging-steel-guide\/","title":{"rendered":"\u0420\u0443\u043a\u043e\u0432\u043e\u0434\u0441\u0442\u0432\u043e \u043f\u043e \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u043e-\u0441\u0442\u0430\u0440\u0435\u044e\u0449\u0435\u0439 \u0441\u0442\u0430\u043b\u0438"},"content":{"rendered":"<p class=\"c4 wp-block-paragraph\"><span class=\"c2\">\u041c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u0430\u044f \u0441\u0442\u0430\u043b\u044c \u2014 \u0441\u0435\u043a\u0440\u0435\u0442\u043d\u044b\u0439 \u0433\u0435\u0440\u043e\u0439 \u0440\u0430\u043a\u0435\u0442, \u043c\u0435\u0434\u0438\u0446\u0438\u043d\u0441\u043a\u0438\u0445 \u0438\u043d\u0441\u0442\u0440\u0443\u043c\u0435\u043d\u0442\u043e\u0432 \u0438 \u0441\u0432\u0435\u0440\u0445\u043f\u0440\u043e\u0447\u043d\u044b\u0445 \u043f\u0440\u043e\u043c\u044b\u0448\u043b\u0435\u043d\u043d\u044b\u0445 \u0434\u0435\u0442\u0430\u043b\u0435\u0439. \u0412 \u043e\u0442\u043b\u0438\u0447\u0438\u0435 \u043e\u0442 \u043e\u0431\u044b\u0447\u043d\u043e\u0439 \u0441\u0442\u0430\u043b\u0438, \u043e\u043d\u0430 \u043f\u0440\u0438\u043e\u0431\u0440\u0435\u0442\u0430\u0435\u0442 \u0441\u0432\u0435\u0440\u0445\u0447\u0435\u043b\u043e\u0432\u0435\u0447\u0435\u0441\u043a\u0443\u044e \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u044c \u0437\u0430 \u0441\u0447\u0435\u0442 \u0441\u043f\u0435\u0446\u0438\u0430\u043b\u044c\u043d\u043e\u0439 \u0442\u0435\u0440\u043c\u0438\u0447\u0435\u0441\u043a\u043e\u0439 \u043e\u0431\u0440\u0430\u0431\u043e\u0442\u043a\u0438, \u0430 \u043d\u0435 \u0443\u0433\u043b\u0435\u0440\u043e\u0434\u0430. <\/span><\/p><p class=\"c4 wp-block-paragraph\"><span class=\"c2\">\u0412 SteelPro Group \u043c\u044b \u043f\u043e\u043c\u043e\u0433\u0430\u0435\u043c \u0438\u043d\u0436\u0435\u043d\u0435\u0440\u0430\u043c \u0438\u0441\u043f\u043e\u043b\u044c\u0437\u043e\u0432\u0430\u0442\u044c \u044d\u0442\u043e\u0442 \u043c\u0430\u0442\u0435\u0440\u0438\u0430\u043b \u0434\u043b\u044f \u0440\u0435\u0448\u0435\u043d\u0438\u044f \u0441\u043b\u043e\u0436\u043d\u044b\u0445 \u0437\u0430\u0434\u0430\u0447 \u0443\u0436\u0435 \u0431\u043e\u043b\u0435\u0435 20 \u043b\u0435\u0442. \u0412 \u044d\u0442\u043e\u0439 \u0441\u0442\u0430\u0442\u044c\u0435 \u0432\u044b \u0443\u0437\u043d\u0430\u0435\u0442\u0435, \u0447\u0442\u043e \u0434\u0435\u043b\u0430\u0435\u0442 \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u0443\u044e \u0441\u0442\u0430\u043b\u044c \u0443\u043d\u0438\u043a\u0430\u043b\u044c\u043d\u043e\u0439, \u0432 \u0447\u0435\u043c \u0435\u0435 \u043f\u0440\u0435\u0438\u043c\u0443\u0449\u0435\u0441\u0442\u0432\u0430 \u0438 \u043a\u0430\u043a \u0441 \u043d\u0435\u0439 \u044d\u0444\u0444\u0435\u043a\u0442\u0438\u0432\u043d\u043e \u0440\u0430\u0431\u043e\u0442\u0430\u0442\u044c<\/span><\/p><h2 class=\"wp-block-heading c4 c8\" id=\"h.sovzh6gsi4ou\"><span class=\"c26\">\u0427\u0442\u043e \u0442\u0430\u043a\u043e\u0435 \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u043e\u0441\u0442\u0430\u0440\u0435\u044e\u0449\u0430\u044f \u0441\u0442\u0430\u043b\u044c?<\/span><\/h2><p class=\"c4 wp-block-paragraph\"><span class=\"c2\">\u041c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u0430\u044f \u0441\u0442\u0430\u043b\u044c \u2014 \u044d\u0442\u043e \u0441\u0432\u0435\u0440\u0445\u043f\u0440\u043e\u0447\u043d\u044b\u0439 \u0441\u043f\u043b\u0430\u0432 \u0441 \u043f\u043e\u0447\u0442\u0438 \u043d\u0443\u043b\u0435\u0432\u044b\u043c \u0441\u043e\u0434\u0435\u0440\u0436\u0430\u043d\u0438\u0435\u043c \u0443\u0433\u043b\u0435\u0440\u043e\u0434\u0430 (&lt;0,03%). \u041e\u043d \u0438\u0437\u0433\u043e\u0442\u043e\u0432\u043b\u0435\u043d \u043d\u0430 \u043e\u0441\u043d\u043e\u0432\u0435 \u0436\u0435\u043b\u0435\u0437\u0430 \u0438 \u043d\u0438\u043a\u0435\u043b\u044f \u0432 \u0441\u043e\u0447\u0435\u0442\u0430\u043d\u0438\u0438 \u0441 \u043a\u043e\u0431\u0430\u043b\u044c\u0442\u043e\u043c, \u043c\u043e\u043b\u0438\u0431\u0434\u0435\u043d\u043e\u043c \u0438 \u0442\u0438\u0442\u0430\u043d\u043e\u043c. \u0412 \u043e\u0442\u043b\u0438\u0447\u0438\u0435 \u043e\u0442 \u043e\u0431\u044b\u0447\u043d\u043e\u0439 \u0441\u0442\u0430\u043b\u0438, \u043a\u043e\u0442\u043e\u0440\u0430\u044f \u0438\u0441\u043f\u043e\u043b\u044c\u0437\u0443\u0435\u0442 \u0443\u0433\u043b\u0435\u0440\u043e\u0434 \u0434\u043b\u044f \u043f\u043e\u043b\u0443\u0447\u0435\u043d\u0438\u044f \u0442\u0432\u0435\u0440\u0434\u043e\u0441\u0442\u0438, \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u0430\u044f \u0441\u0442\u0430\u043b\u044c \u043f\u0440\u0438\u043e\u0431\u0440\u0435\u0442\u0430\u0435\u0442 \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u044c \u043f\u043e\u0441\u0440\u0435\u0434\u0441\u0442\u0432\u043e\u043c \u0442\u0435\u0440\u043c\u0438\u0447\u0435\u0441\u043a\u043e\u0439 \u043e\u0431\u0440\u0430\u0431\u043e\u0442\u043a\u0438. \u0412\u043e \u0432\u0440\u0435\u043c\u044f \u044d\u0442\u043e\u0433\u043e \u043f\u0440\u043e\u0446\u0435\u0441\u0441\u0430 \u043e\u0431\u0440\u0430\u0437\u0443\u044e\u0442\u0441\u044f \u043a\u0440\u043e\u0448\u0435\u0447\u043d\u044b\u0435 \u0447\u0430\u0441\u0442\u0438\u0446\u044b, \u0442\u0430\u043a\u0438\u0435 \u043a\u0430\u043a Ni\u2083Mo, \u043a\u043e\u0442\u043e\u0440\u044b\u0435 \u0441\u043a\u0440\u0435\u043f\u043b\u044f\u044e\u0442 \u0441\u0442\u0440\u0443\u043a\u0442\u0443\u0440\u0443. \u042d\u0442\u043e \u0438\u0437\u0432\u0435\u0441\u0442\u043d\u043e \u043a\u0430\u043a \u00ab\u0441\u0442\u0430\u0440\u0435\u043d\u0438\u0435\u00bb.<\/span><\/p><p class=\"c4 wp-block-paragraph\"><span class=\"c2\">\u0412 \u0441\u044b\u0440\u043e\u043c \u0432\u0438\u0434\u0435 \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u0430\u044f \u0441\u0442\u0430\u043b\u044c \u0434\u043e\u0441\u0442\u0430\u0442\u043e\u0447\u043d\u043e \u043c\u044f\u0433\u043a\u0430\u044f, \u0447\u0442\u043e\u0431\u044b \u0435\u0435 \u043c\u043e\u0436\u043d\u043e \u0431\u044b\u043b\u043e \u043b\u0435\u0433\u043a\u043e \u0440\u0435\u0437\u0430\u0442\u044c \u0438\u043b\u0438 \u0444\u043e\u0440\u043c\u043e\u0432\u0430\u0442\u044c, \u0441 \u0442\u0432\u0435\u0440\u0434\u043e\u0441\u0442\u044c\u044e RC30-35. \u041d\u043e \u043f\u043e\u0441\u043b\u0435 \u0441\u0442\u0430\u0440\u0435\u043d\u0438\u044f \u043e\u043d\u0430 \u043f\u0440\u0435\u0432\u0440\u0430\u0449\u0430\u0435\u0442\u0441\u044f \u0432 \u043d\u0435\u0432\u0435\u0440\u043e\u044f\u0442\u043d\u043e \u043f\u0440\u043e\u0447\u043d\u044b\u0439 \u0438 \u0443\u0434\u0430\u0440\u043e\u043f\u0440\u043e\u0447\u043d\u044b\u0439 \u043c\u0430\u0442\u0435\u0440\u0438\u0430\u043b. \u042d\u0442\u043e \u0434\u0435\u043b\u0430\u0435\u0442 \u0435\u0435 \u0438\u0434\u0435\u0430\u043b\u044c\u043d\u043e\u0439 \u0434\u043b\u044f:<\/span><\/p><ul class=\"wp-block-list c14 lst-kix_dpv1gn83yrv8-0 start\"><li><span class=\"c2\">\u0414\u0435\u0442\u0430\u043b\u0438 \u0430\u044d\u0440\u043e\u043a\u043e\u0441\u043c\u0438\u0447\u0435\u0441\u043a\u043e\u0439 \u0442\u0435\u0445\u043d\u0438\u043a\u0438, \u0442\u0440\u0435\u0431\u0443\u044e\u0449\u0438\u0435 \u043b\u0435\u0433\u043a\u043e\u0441\u0442\u0438 \u0438 \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u0438<\/span><\/li>\n\n<li><span class=\"c2\">\u041f\u0440\u0435\u0446\u0438\u0437\u0438\u043e\u043d\u043d\u044b\u0435 \u0444\u043e\u0440\u043c\u044b, \u0442\u0440\u0435\u0431\u0443\u044e\u0449\u0438\u0435 \u0442\u043e\u0447\u043d\u044b\u0445 \u0444\u043e\u0440\u043c<\/span><\/li>\n\n<li><span class=\"c2\">\u041a\u0440\u0438\u0442\u0438\u0447\u0435\u0441\u043a\u0438\u0435 \u043a\u043e\u043c\u043f\u043e\u043d\u0435\u043d\u0442\u044b, \u043e\u0442\u043a\u0430\u0437 \u043a\u043e\u0442\u043e\u0440\u044b\u0445 \u043d\u0435\u0434\u043e\u043f\u0443\u0441\u0442\u0438\u043c<\/span><\/li><\/ul><h3 class=\"wp-block-heading c4 c8\" id=\"h.7gikto4owsc9\"><span class=\"c17\">\u041f\u043e\u0447\u0435\u043c\u0443 \u0442\u0430\u043a\u043e\u0435 \u043d\u0430\u0437\u0432\u0430\u043d\u0438\u0435?<\/span><\/h3><ul class=\"wp-block-list c14 lst-kix_dwsuylhjhclw-0 start\"><li><span class=\"c2\">\u00ab\u041c\u0430\u0440\u00bb = \u041c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442: \u043f\u0435\u0440\u0432\u043e\u043d\u0430\u0447\u0430\u043b\u044c\u043d\u0430\u044f \u043f\u0440\u043e\u0447\u043d\u0430\u044f, \u043d\u043e \u0440\u0430\u0431\u043e\u0442\u043e\u0441\u043f\u043e\u0441\u043e\u0431\u043d\u0430\u044f \u0441\u0442\u0440\u0443\u043a\u0442\u0443\u0440\u0430.<\/span><\/li>\n\n<li><span class=\"c2\">\u00ab\u0421\u0442\u0430\u0440\u0435\u043d\u0438\u0435\u00bb = \u0414\u043b\u0438\u0442\u0435\u043b\u044c\u043d\u0430\u044f \u0442\u0435\u0440\u043c\u043e\u043e\u0431\u0440\u0430\u0431\u043e\u0442\u043a\u0430, \u0441\u043e\u0445\u0440\u0430\u043d\u044f\u044e\u0449\u0430\u044f \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u044c.<\/span><\/li><\/ul><h2 class=\"wp-block-heading c34\" id=\"h.7398zygjosas\"><span class=\"c26\">\u041a\u043b\u044e\u0447\u0435\u0432\u044b\u0435 \u0445\u0430\u0440\u0430\u043a\u0442\u0435\u0440\u0438\u0441\u0442\u0438\u043a\u0438 \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u043e\u0441\u0442\u0430\u0440\u0435\u044e\u0449\u0435\u0439 \u0441\u0442\u0430\u043b\u0438<\/span><\/h2><ul class=\"wp-block-list c14 lst-kix_3uv51juinlpg-0 start\"><li><span class=\"c5\">\u0427\u0435\u043c\u043f\u0438\u043e\u043d \u043f\u043e \u0441\u0438\u043b\u0435 \u0438 \u0432\u0435\u0441\u0443<\/span><span class=\"c2\">: \u041f\u0440\u0435\u0432\u043e\u0441\u0445\u043e\u0434\u0438\u0442 \u0442\u0438\u0442\u0430\u043d\u043e\u0432\u044b\u0435 \u0441\u043f\u043b\u0430\u0432\u044b \u0432 \u0443\u0441\u043b\u043e\u0432\u0438\u044f\u0445 \u043d\u0430\u0433\u0440\u0443\u0437\u043a\u0438.<\/span><\/li>\n\n<li><span class=\"c5\">\u0422\u0435\u0440\u043c\u0438\u0447\u0435\u0441\u043a\u0430\u044f \u0441\u0442\u0430\u0431\u0438\u043b\u044c\u043d\u043e\u0441\u0442\u044c<\/span><span class=\"c2\">: \u0421\u043e\u0445\u0440\u0430\u043d\u044f\u0435\u0442 \u0442\u043e\u0447\u043d\u044b\u0435 \u0440\u0430\u0437\u043c\u0435\u0440\u044b \u0432\u043e \u0432\u0440\u0435\u043c\u044f \u0441\u0442\u0430\u0440\u0435\u043d\u0438\u044f.<\/span><\/li>\n\n<li><span class=\"c5\">\u0423\u0441\u0442\u043e\u0439\u0447\u0438\u0432\u043e\u0441\u0442\u044c \u043a \u0442\u0440\u0435\u0449\u0438\u043d\u0430\u043c<\/span><span class=\"c2\">: \u0412\u044b\u0434\u0435\u0440\u0436\u0438\u0432\u0430\u0435\u0442 \u0443\u0434\u0430\u0440\u043d\u044b\u0435 \u043d\u0430\u0433\u0440\u0443\u0437\u043a\u0438 \u043b\u0443\u0447\u0448\u0435, \u0447\u0435\u043c \u0431\u043e\u043b\u044c\u0448\u0438\u043d\u0441\u0442\u0432\u043e \u0432\u044b\u0441\u043e\u043a\u043e\u043f\u0440\u043e\u0447\u043d\u044b\u0445 \u0441\u043f\u043b\u0430\u0432\u043e\u0432, \u0434\u0430\u0436\u0435 \u043f\u0440\u0438 \u043e\u0442\u0440\u0438\u0446\u0430\u0442\u0435\u043b\u044c\u043d\u044b\u0445 \u0442\u0435\u043c\u043f\u0435\u0440\u0430\u0442\u0443\u0440\u0430\u0445.<\/span><\/li>\n\n<li><span class=\"c5\">\u0417\u0430\u0449\u0438\u0442\u0430 \u043e\u0442 \u043a\u043e\u0440\u0440\u043e\u0437\u0438\u0438<\/span><span class=\"c2\">: \u0421\u043e\u0431\u0441\u0442\u0432\u0435\u043d\u043d\u0430\u044f \u0441\u0442\u043e\u0439\u043a\u043e\u0441\u0442\u044c \u043a \u0432\u043e\u0434\u043e\u0440\u043e\u0434\u043d\u043e\u043c\u0443 \u043e\u0445\u0440\u0443\u043f\u0447\u0438\u0432\u0430\u043d\u0438\u044e \u0438 \u043a\u043e\u0440\u0440\u043e\u0437\u0438\u043e\u043d\u043d\u043e\u043c\u0443 \u0440\u0430\u0441\u0442\u0440\u0435\u0441\u043a\u0438\u0432\u0430\u043d\u0438\u044e \u043f\u043e\u0434 \u043d\u0430\u043f\u0440\u044f\u0436\u0435\u043d\u0438\u0435\u043c.<\/span><\/li>\n\n<li><span class=\"c5\">\u041c\u044f\u0433\u043a\u0438\u0439 \u0441\u0442\u043e\u043b\u0438\u043a, \u0443\u0434\u043e\u0431\u043d\u044b\u0439 \u0434\u043b\u044f \u043e\u0431\u0440\u0430\u0431\u043e\u0442\u043a\u0438<\/span><span class=\"c2\">: \u041b\u0435\u0433\u043a\u043e \u0444\u043e\u0440\u043c\u0443\u0435\u0442\u0441\u044f\/\u0440\u0435\u0436\u0435\u0442\u0441\u044f \u0432 \u043e\u0442\u043e\u0436\u0436\u0435\u043d\u043d\u043e\u043c \u0441\u043e\u0441\u0442\u043e\u044f\u043d\u0438\u0438 (\u0434\u043e \u0441\u0442\u0430\u0440\u0435\u043d\u0438\u044f).<\/span><\/li>\n\n<li><span class=\"c5\">\u0421\u0432\u0430\u0440\u0438\u0432\u0430\u0435\u043c\u044b\u0439 \u0431\u0435\u0437 \u043f\u0440\u0435\u0434\u0432\u0430\u0440\u0438\u0442\u0435\u043b\u044c\u043d\u043e\u0433\u043e \u043d\u0430\u0433\u0440\u0435\u0432\u0430<\/span><span class=\"c2\">: \u043f\u043e\u0437\u0432\u043e\u043b\u044f\u0435\u0442 \u043f\u0440\u043e\u0438\u0437\u0432\u043e\u0434\u0438\u0442\u044c \u0440\u0435\u043c\u043e\u043d\u0442 \u043d\u0430 \u043c\u0435\u0441\u0442\u0435 \u2014 \u0440\u0435\u0434\u043a\u0430\u044f \u043e\u0441\u043e\u0431\u0435\u043d\u043d\u043e\u0441\u0442\u044c \u0441\u0440\u0435\u0434\u0438 \u0441\u0432\u0435\u0440\u0445\u043f\u0440\u043e\u0447\u043d\u044b\u0445 \u043c\u0435\u0442\u0430\u043b\u043b\u043e\u0432.<\/span><\/li><\/ul><h2 class=\"wp-block-heading c4 c8\" id=\"h.x5mib7akpys8\"><span class=\"c26\">\u041a\u0440\u0430\u0442\u043a\u0438\u0439 \u043e\u0431\u0437\u043e\u0440 \u043c\u0430\u0440\u043e\u043a \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u043e\u0441\u0442\u0430\u0440\u0435\u044e\u0449\u0435\u0439 \u0441\u0442\u0430\u043b\u0438<\/span><\/h2><figure class=\"wp-block-table\"><table><tbody><tr><td><strong>\u041e\u0446\u0435\u043d\u043a\u0430<\/strong><\/td><td><strong>\u0421\u0442\u0430\u043d\u0434\u0430\u0440\u0442 \u0410\u041c\u0421<\/strong><\/td><td><strong>\u041f\u0440\u0435\u0434\u0435\u043b \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u0438<\/strong><\/td><td><strong>\u0421\u043e\u0434\u0435\u0440\u0436\u0430\u043d\u0438\u0435 \u043a\u043e\u0431\u0430\u043b\u044c\u0442\u0430<\/strong><\/td><td><strong>\u0421\u043e\u0434\u0435\u0440\u0436\u0430\u043d\u0438\u0435 \u0442\u0438\u0442\u0430\u043d\u0430<\/strong><\/td><td><strong>\u0422\u0438\u043f\u0438\u0447\u043d\u044b\u0435 \u043f\u0440\u0438\u043c\u0435\u043d\u0435\u043d\u0438\u044f<\/strong><\/td><\/tr><tr><td>\u0421200<\/td><td>\u0410\u041c\u0421 6511<\/td><td>1380 \u041c\u041f\u0430<\/td><td>8-9%<\/td><td>0.15-0.25%<\/td><td>\u0424\u043e\u0440\u043c\u044b \u0434\u043b\u044f \u043b\u0438\u0442\u044c\u044f \u043f\u043e\u0434 \u0434\u0430\u0432\u043b\u0435\u043d\u0438\u0435\u043c, \u0441\u0442\u0440\u0443\u043a\u0442\u0443\u0440\u043d\u044b\u0435 \u043a\u0440\u043e\u043d\u0448\u0442\u0435\u0439\u043d\u044b<\/td><\/tr><tr><td>\u0421250<\/td><td>\u0410\u041c\u0421 6512<\/td><td>1720 \u041c\u041f\u0430<\/td><td>7-8.5%<\/td><td>0.3-0.5%<\/td><td>\u0410\u044d\u0440\u043e\u043a\u043e\u0441\u043c\u0438\u0447\u0435\u0441\u043a\u0438\u0435 \u043f\u0440\u0438\u0432\u043e\u0434\u044b, \u0433\u0438\u0434\u0440\u0430\u0432\u043b\u0438\u0447\u0435\u0441\u043a\u0438\u0435 \u0441\u0438\u0441\u0442\u0435\u043c\u044b<\/td><\/tr><tr><td>\u0421300<\/td><td>\u0410\u041c\u0421 6514<\/td><td>2070 \u041c\u041f\u0430<\/td><td>8.5-9.5%<\/td><td>0.5-0.8%<\/td><td>\u041a\u043e\u0440\u043f\u0443\u0441\u0430 \u0440\u0430\u043a\u0435\u0442\u043d\u044b\u0445 \u0434\u0432\u0438\u0433\u0430\u0442\u0435\u043b\u0435\u0439, \u044d\u043a\u0441\u0442\u0440\u0443\u0437\u0438\u043e\u043d\u043d\u044b\u0435 \u043c\u0430\u0442\u0440\u0438\u0446\u044b<\/td><\/tr><tr><td>\u0421350<\/td><td>\u0410\u041c\u0421 6515*<\/td><td>2410 \u041c\u041f\u0430<\/td><td>11.5-12.5%<\/td><td>1.3-1.6%<\/td><td>\u042f\u0434\u0435\u0440\u043d\u044b\u0435 \u0446\u0435\u043d\u0442\u0440\u0438\u0444\u0443\u0433\u0438, \u0432\u043e\u0435\u043d\u043d\u044b\u0435 \u043a\u043e\u043c\u043f\u043e\u043d\u0435\u043d\u0442\u044b<\/td><\/tr><tr><td colspan=\"6\">*C350 \u0442\u0440\u0435\u0431\u0443\u0435\u0442 \u044d\u043a\u0441\u043f\u043e\u0440\u0442\u043d\u044b\u0445 \u043b\u0438\u0446\u0435\u043d\u0437\u0438\u0439 \u0432 \u0441\u043e\u043e\u0442\u0432\u0435\u0442\u0441\u0442\u0432\u0438\u0438 \u0441 \u0441\u043e\u0433\u043b\u0430\u0448\u0435\u043d\u0438\u044f\u043c\u0438 \u043e \u043d\u0435\u0440\u0430\u0441\u043f\u0440\u043e\u0441\u0442\u0440\u0430\u043d\u0435\u043d\u0438\u0438 \u044f\u0434\u0435\u0440\u043d\u043e\u0433\u043e \u043e\u0440\u0443\u0436\u0438\u044f.<\/td><\/tr><\/tbody><\/table><\/figure><p class=\"c4 wp-block-paragraph\"><span class=\"c2\">\u0412\u0441\u0435 \u043c\u0430\u0440\u043a\u0438 \u043f\u0440\u043e\u0445\u043e\u0434\u044f\u0442 \u0441\u0442\u0440\u043e\u0433\u0443\u044e \u0432\u0430\u043a\u0443\u0443\u043c\u043d\u0443\u044e \u043f\u043b\u0430\u0432\u043a\u0443 (VIM\/VAR) \u0434\u043b\u044f \u043c\u0438\u043d\u0438\u043c\u0438\u0437\u0430\u0446\u0438\u0438 \u043f\u0440\u0438\u043c\u0435\u0441\u0435\u0439. \u0412 SteelPro Group \u043c\u044b \u043f\u043e\u043c\u043e\u0433\u0430\u0435\u043c \u043a\u043b\u0438\u0435\u043d\u0442\u0430\u043c \u0432\u044b\u0431\u0438\u0440\u0430\u0442\u044c \u043e\u043f\u0442\u0438\u043c\u0430\u043b\u044c\u043d\u0443\u044e \u043c\u0430\u0440\u043a\u0443 \u043d\u0430 \u043e\u0441\u043d\u043e\u0432\u0435 \u0441\u0442\u043e\u0438\u043c\u043e\u0441\u0442\u0438, \u043f\u0440\u043e\u0438\u0437\u0432\u043e\u0434\u0441\u0442\u0432\u0435\u043d\u043d\u044b\u0445 \u043f\u043e\u0442\u0440\u0435\u0431\u043d\u043e\u0441\u0442\u0435\u0439 \u0438 \u0442\u0440\u0435\u0431\u043e\u0432\u0430\u043d\u0438\u0439 \u043a\u043e\u043d\u0435\u0447\u043d\u043e\u0433\u043e \u043f\u043e\u043b\u044c\u0437\u043e\u0432\u0430\u0442\u0435\u043b\u044f.<\/span><\/p><h2 class=\"wp-block-heading c4 c8\" id=\"h.ei826o403ifj\"><span class=\"c26\">\u0425\u0438\u043c\u0438\u0447\u0435\u0441\u043a\u0438\u0439 \u0441\u043e\u0441\u0442\u0430\u0432 \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u043e\u0441\u0442\u0430\u0440\u0435\u044e\u0449\u0435\u0439 \u0441\u0442\u0430\u043b\u0438<\/span><\/h2><figure class=\"wp-block-table\"><table><tbody><tr><td><strong>\u041e\u0446\u0435\u043d\u043a\u0438<\/strong><\/td><td><strong>\u0421200<\/strong><\/td><td><strong>\u0421250<\/strong><\/td><td><strong>\u0421300<\/strong><\/td><td><strong>\u0421350<\/strong><\/td><\/tr><tr><td><strong>\u041d\u0438\u043a\u0435\u043b\u044c (Ni)<\/strong><\/td><td>17,0\u201319,0<\/td><td>17,0\u201319,0<\/td><td>18,0\u201319,0<\/td><td>18,0\u201319,0<\/td><\/tr><tr><td><strong>\u041a\u043e\u0431\u0430\u043b\u044c\u0442 (Co)<\/strong><\/td><td>8,0\u20139,0<\/td><td>7,0\u20138,5<\/td><td>8,5\u20139,5<\/td><td>11,5\u201312,5<\/td><\/tr><tr><td><strong>\u041c\u043e\u043b\u0438\u0431\u0434\u0435\u043d (Mo)<\/strong><\/td><td>3,0\u20133,5<\/td><td>4.6\u20135.2<\/td><td>4.6\u20135.2<\/td><td>4.6\u20135.2<\/td><\/tr><tr><td><strong>\u0422\u0438\u0442\u0430\u043d (Ti)<\/strong><\/td><td>0,15\u20130,25<\/td><td>0,3\u20130,5<\/td><td>0,5\u20130,8<\/td><td>1,3\u20131,6<\/td><\/tr><tr><td><strong>\u0410\u043b\u044e\u043c\u0438\u043d\u0438\u0439 (Al)<\/strong><\/td><td>0,05\u20130,15<\/td><td>0,05\u20130,15<\/td><td>0,05\u20130,15<\/td><td>0,05\u20130,15<\/td><\/tr><tr><td><strong>\u0423\u0433\u043b\u0435\u0440\u043e\u0434 (\u0421)<\/strong><\/td><td>\u22640,03<\/td><td>\u22640,03<\/td><td>\u22640,03<\/td><td>\u22640,03<\/td><\/tr><tr><td><strong>\u041a\u0440\u0435\u043c\u043d\u0438\u0439 (Si)<\/strong><\/td><td>\u22640,10<\/td><td>\u22640,10<\/td><td>\u22640,10<\/td><td>\u22640,10<\/td><\/tr><tr><td><strong>\u041c\u0430\u0440\u0433\u0430\u043d\u0435\u0446 (Mn)<\/strong><\/td><td>\u22640,10<\/td><td>\u22640,10<\/td><td>\u22640,10<\/td><td>\u22640,10<\/td><\/tr><tr><td><strong>\u0416\u0435\u043b\u0435\u0437\u043e (Fe)<\/strong><\/td><td>\u0411\u0430\u043b\u0430\u043d\u0441<\/td><td>\u0411\u0430\u043b\u0430\u043d\u0441<\/td><td>\u0411\u0430\u043b\u0430\u043d\u0441<\/td><td>\u0411\u0430\u043b\u0430\u043d\u0441<\/td><\/tr><\/tbody><\/table><\/figure><h2 class=\"wp-block-heading c4 c8\" id=\"h.aoaybovkfuj0\"><span class=\"c26\">\u041c\u0435\u0445\u0430\u043d\u0438\u0447\u0435\u0441\u043a\u0438\u0435 \u0441\u0432\u043e\u0439\u0441\u0442\u0432\u0430 \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u043e\u0441\u0442\u0430\u0440\u0435\u044e\u0449\u0435\u0439 \u0441\u0442\u0430\u043b\u0438<\/span><\/h2><figure class=\"wp-block-table\"><table><tbody><tr><td><strong>\u0421\u0432\u043e\u0439\u0441\u0442\u0432\u043e<\/strong><\/td><td><strong>\u0421200<\/strong><\/td><td><strong>\u0421250<\/strong><\/td><td><strong>\u0421300<\/strong><\/td><td><strong>\u0421350<\/strong><\/td><\/tr><tr><td><strong>\u041f\u0440\u0435\u0434\u0435\u043b \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u0438<\/strong><\/td><td>1379 \u041c\u041f\u0430 (200 \u0442\u044b\u0441.\u0444\u0443\u043d\u0442\u043e\u0432\/\u043a\u0432.\u0434\u044e\u0439\u043c)<\/td><td>1724 \u041c\u041f\u0430 (250 \u0442\u044b\u0441.\u0444\u0443\u043d\u0442\u043e\u0432\/\u043a\u0432.\u0434\u044e\u0439\u043c)<\/td><td>2068 \u041c\u041f\u0430 (300 \u0442\u044b\u0441.\u0444\u0443\u043d\u0442\u043e\u0432\/\u043a\u0432.\u0434\u044e\u0439\u043c)<\/td><td>2413 \u041c\u041f\u0430 (350 \u0442\u044b\u0441.\u0444\u0443\u043d\u0442\u043e\u0432\/\u043a\u0432.\u0434\u044e\u0439\u043c)<\/td><\/tr><tr><td><strong>\u041f\u0440\u0435\u0434\u0435\u043b \u0442\u0435\u043a\u0443\u0447\u0435\u0441\u0442\u0438 (0,2%)<\/strong><\/td><td>1724 \u041c\u041f\u0430 (250 \u0442\u044b\u0441.\u0444\u0443\u043d\u0442\u043e\u0432\/\u043a\u0432.\u0434\u044e\u0439\u043c)<\/td><td>1930 \u041c\u041f\u0430 (280 \u0442\u044b\u0441.\u0444\u0443\u043d\u0442\u043e\u0432\/\u043a\u0432.\u0434\u044e\u0439\u043c)<\/td><td>2275 \u041c\u041f\u0430 (330 \u0442\u044b\u0441.\u0444\u0443\u043d\u0442\u043e\u0432\/\u043a\u0432.\u0434\u044e\u0439\u043c)<\/td><td>2620 \u041c\u041f\u0430 (380 \u0442\u044b\u0441.\u0444\u0443\u043d\u0442\u043e\u0432\/\u043a\u0432.\u0434\u044e\u0439\u043c)<\/td><\/tr><tr><td><strong>\u0423\u0434\u043b\u0438\u043d\u0435\u043d\u0438\u0435 (%)<\/strong><\/td><td>11\u201315%<\/td><td>10\u2013121\u0422\u04203\u0422<\/td><td>8\u201310%<\/td><td>6\u20138%<\/td><\/tr><tr><td><strong>\u0423\u043c\u0435\u043d\u044c\u0448\u0435\u043d\u0438\u0435 \u043f\u043b\u043e\u0449\u0430\u0434\u0438 (%)<\/strong><\/td><td>50\u201360%<\/td><td>45\u201355%<\/td><td>40\u201350%<\/td><td>25\u201335%<\/td><\/tr><tr><td><strong>\u0422\u0432\u0435\u0440\u0434\u043e\u0441\u0442\u044c (\u0441\u043e\u0441\u0442\u0430\u0440\u0435\u043d\u043d\u0430\u044f, HRC)<\/strong><\/td><td>30\u201335 HRC<\/td><td>50 HRC<\/td><td>54 HRC<\/td><td>58 \u0427\u0420\u0421<\/td><\/tr><tr><td><strong>\u0412\u044f\u0437\u043a\u043e\u0441\u0442\u044c \u0440\u0430\u0437\u0440\u0443\u0448\u0435\u043d\u0438\u044f (KIC)<\/strong><\/td><td>175 \u041c\u041f\u0430\u00b7\u043c\u00b9\u2044\u00b2 (160 ksi\u221ain)<\/td><td>&#8211;<\/td><td>&#8211;<\/td><td>&#8211;<\/td><\/tr><\/tbody><\/table><\/figure><h2 class=\"wp-block-heading c4 c8\" id=\"h.cjj6q62rl3h\"><span class=\"c26\">\u0424\u0438\u0437\u0438\u0447\u0435\u0441\u043a\u0438\u0435 \u0441\u0432\u043e\u0439\u0441\u0442\u0432\u0430 \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u043e\u0441\u0442\u0430\u0440\u0435\u044e\u0449\u0435\u0439 \u0441\u0442\u0430\u043b\u0438<\/span><\/h2><figure class=\"wp-block-table\"><table><tbody><tr><td><strong>\u0421\u0432\u043e\u0439\u0441\u0442\u0432\u043e<\/strong><\/td><td><strong>\u041c\u0435\u0442\u0440\u0438\u0447\u0435\u0441\u043a\u0438\u0435 \u0435\u0434\u0438\u043d\u0438\u0446\u044b<\/strong><\/td><td><strong>\u0418\u043c\u043f\u0435\u0440\u0441\u043a\u0438\u0435 \u0435\u0434\u0438\u043d\u0438\u0446\u044b<\/strong><\/td><\/tr><tr><td><strong>\u041f\u043b\u043e\u0442\u043d\u043e\u0441\u0442\u044c<\/strong><\/td><td>8,1 \u0433\/\u0441\u043c\u00b3<\/td><td>0,292 \u0444\u0443\u043d\u0442\u0430\/\u0434\u044e\u0439\u043c\u00b3<\/td><\/tr><tr><td><strong>\u0422\u0435\u043c\u043f\u0435\u0440\u0430\u0442\u0443\u0440\u0430 \u043f\u043b\u0430\u0432\u043b\u0435\u043d\u0438\u044f<\/strong><\/td><td>1413\u00b0\u0421<\/td><td>2575\u00b0F<\/td><\/tr><tr><td><strong>\u0422\u0435\u043f\u043b\u043e\u043f\u0440\u043e\u0432\u043e\u0434\u043d\u043e\u0441\u0442\u044c<\/strong><\/td><td>25,5 \u0412\u0442\/\u043c\u00b7\u041a<\/td><td>17,7 \u0411\u0422\u0415\u00b7\u0434\u044e\u0439\u043c\/\u0447\u00b7\u0444\u0443\u0442\u00b2\u00b7\u00b0F<\/td><\/tr><tr><td><strong>\u041a\u043e\u044d\u0444\u0444\u0438\u0446\u0438\u0435\u043d\u0442 \u0442\u0435\u043f\u043b\u043e\u0432\u043e\u0433\u043e \u0440\u0430\u0441\u0448\u0438\u0440\u0435\u043d\u0438\u044f<\/strong><\/td><td>11,3\u00d710\u207b\u2076 K\u207b\u00b9 (20\u2013100\u00b0C)<\/td><td>6,3\u00d710\u207b\u2076 \u0434\u044e\u0439\u043c\/\u0434\u044e\u0439\u043c\u00b7\u00b0F (68\u2013212\u00b0F)<\/td><\/tr><tr><td><strong>\u0423\u0434\u0435\u043b\u044c\u043d\u0430\u044f \u0442\u0435\u043f\u043b\u043e\u0435\u043c\u043a\u043e\u0441\u0442\u044c<\/strong><\/td><td>452 \u0414\u0436\/\u043a\u0433\u00b7\u041a<\/td><td>0,108 \u0411\u0422\u0415\/\u0444\u0443\u043d\u0442\u00b7\u00b0F<\/td><\/tr><tr><td><strong>\u041c\u043e\u0434\u0443\u043b\u044c \u042e\u043d\u0433\u0430<\/strong><\/td><td>210 \u0413\u041f\u0430<\/td><td>30\u00d710\u2076 \u0444\u0443\u043d\u0442\u043e\u0432 \u043d\u0430 \u043a\u0432. \u0434\u044e\u0439\u043c<\/td><\/tr><tr><td><strong>\u041c\u043e\u0434\u0443\u043b\u044c \u0441\u0434\u0432\u0438\u0433\u0430<\/strong><\/td><td>77 \u0413\u041f\u0430<\/td><td>11,2\u00d710\u2076 \u0444\u0443\u043d\u0442\u043e\u0432 \u043d\u0430 \u043a\u0432. \u0434\u044e\u0439\u043c<\/td><\/tr><\/tbody><\/table><\/figure><h2 class=\"wp-block-heading c34\" id=\"h.syd4m5ybpl6\">\u041c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u0430\u044f \u0441\u0442\u0430\u043b\u044c<span class=\"c26\">&nbsp;\u041f\u0440\u0438\u043b\u043e\u0436\u0435\u043d\u0438\u044f<\/span><\/h2><p class=\"c4 wp-block-paragraph\"><span class=\"c28 c5\">1. \u0410\u044d\u0440\u043e\u043a\u043e\u0441\u043c\u0438\u0447\u0435\u0441\u043a\u0430\u044f \u043f\u0440\u043e\u043c\u044b\u0448\u043b\u0435\u043d\u043d\u043e\u0441\u0442\u044c \u0438 \u0430\u0432\u0438\u0430\u0446\u0438\u044f<\/span><\/p><ul class=\"wp-block-list c14 lst-kix_r7ph7cxbu89z-0 start\"><li><span class=\"c2\">\u041a\u043e\u043d\u0441\u0442\u0440\u0443\u043a\u0442\u0438\u0432\u043d\u044b\u0435 \u044d\u043b\u0435\u043c\u0435\u043d\u0442\u044b: \u043a\u043e\u0440\u043f\u0443\u0441\u0430 \u0440\u0430\u043a\u0435\u0442\u043d\u044b\u0445 \u0434\u0432\u0438\u0433\u0430\u0442\u0435\u043b\u0435\u0439, \u043b\u0435\u0433\u043a\u0438\u0435 \u0434\u0435\u0442\u0430\u043b\u0438 \u043f\u043b\u0430\u043d\u0435\u0440\u0430, \u0448\u0430\u0441\u0441\u0438.<\/span><\/li>\n\n<li><span class=\"c2\">\u0421\u0438\u0441\u0442\u0435\u043c\u044b \u0434\u0432\u0438\u0433\u0430\u0442\u0435\u043b\u044f: \u0432\u044b\u0441\u043e\u043a\u043e\u043d\u0430\u0433\u0440\u0443\u0436\u0435\u043d\u043d\u044b\u0435 \u0432\u0430\u043b\u044b \u0442\u0443\u0440\u0431\u0438\u043d, \u0448\u0435\u0441\u0442\u0435\u0440\u043d\u0438 \u0438 \u043a\u0440\u0435\u043f\u0435\u0436\u043d\u044b\u0435 \u044d\u043b\u0435\u043c\u0435\u043d\u0442\u044b.<\/span><\/li>\n\n<li><span class=\"c2\">\u0421\u043f\u0443\u0442\u043d\u0438\u043a\u043e\u0432\u043e\u0435 \u043e\u0431\u043e\u0440\u0443\u0434\u043e\u0432\u0430\u043d\u0438\u0435: \u043f\u0440\u0435\u0446\u0438\u0437\u0438\u043e\u043d\u043d\u044b\u0435 \u0434\u0435\u0442\u0430\u043b\u0438, \u0442\u0440\u0435\u0431\u0443\u044e\u0449\u0438\u0435 \u0432\u044b\u0441\u043e\u043a\u043e\u0433\u043e \u0441\u043e\u043e\u0442\u043d\u043e\u0448\u0435\u043d\u0438\u044f \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u0438 \u0438 \u0432\u0435\u0441\u0430.<\/span><\/li><\/ul><p class=\"c4 wp-block-paragraph\"><span class=\"c28 c5\">2. \u0418\u043d\u0441\u0442\u0440\u0443\u043c\u0435\u043d\u0442\u044b \u0438 \u0448\u0442\u0430\u043c\u043f\u044b<\/span><\/p><ul class=\"wp-block-list c14 lst-kix_u46p9drtji9s-0 start\"><li><span class=\"c2\">\u0424\u043e\u0440\u043c\u044b \u0434\u043b\u044f \u043b\u0438\u0442\u044c\u044f \u043f\u043e\u0434 \u0434\u0430\u0432\u043b\u0435\u043d\u0438\u0435\u043c: \u043f\u043e\u0432\u044b\u0448\u0435\u043d\u043d\u0430\u044f \u0438\u0437\u043d\u043e\u0441\u043e\u0441\u0442\u043e\u0439\u043a\u043e\u0441\u0442\u044c \u0434\u043b\u044f \u043a\u0440\u0443\u043f\u043d\u043e\u0441\u0435\u0440\u0438\u0439\u043d\u043e\u0433\u043e \u043f\u0440\u043e\u0438\u0437\u0432\u043e\u0434\u0441\u0442\u0432\u0430.<\/span><\/li>\n\n<li><span class=\"c2\">\u042d\u043a\u0441\u0442\u0440\u0443\u0437\u0438\u043e\u043d\u043d\u044b\u0435 \u043c\u0430\u0442\u0440\u0438\u0446\u044b: \u041f\u0440\u0435\u0432\u043e\u0441\u0445\u043e\u0434\u043d\u0430\u044f \u0441\u0442\u043e\u0439\u043a\u043e\u0441\u0442\u044c \u043a \u0442\u0435\u0440\u043c\u0438\u0447\u0435\u0441\u043a\u043e\u0439 \u0443\u0441\u0442\u0430\u043b\u043e\u0441\u0442\u0438 \u043f\u0440\u0438 \u0444\u043e\u0440\u043c\u043e\u0432\u0430\u043d\u0438\u0438 \u043c\u0435\u0442\u0430\u043b\u043b\u043e\u0432.<\/span><\/li>\n\n<li><span class=\"c2\">\u041a\u0443\u0437\u043d\u0435\u0447\u043d\u044b\u0439 \u0438\u043d\u0441\u0442\u0440\u0443\u043c\u0435\u043d\u0442: \u0441\u043e\u0445\u0440\u0430\u043d\u044f\u0435\u0442 \u0442\u0432\u0435\u0440\u0434\u043e\u0441\u0442\u044c \u043f\u0440\u0438 \u044d\u043a\u0441\u0442\u0440\u0435\u043c\u0430\u043b\u044c\u043d\u044b\u0445 \u0446\u0438\u043a\u043b\u0438\u0447\u0435\u0441\u043a\u0438\u0445 \u043d\u0430\u0433\u0440\u0443\u0437\u043a\u0430\u0445.<\/span><\/li><\/ul><p class=\"c4 wp-block-paragraph\"><span class=\"c28 c5\">3. \u041e\u0431\u043e\u0440\u043e\u043d\u0430 \u0438 \u0430\u0440\u043c\u0438\u044f<\/span><\/p><ul class=\"wp-block-list c14 lst-kix_s72udy395ak6-0 start\"><li><span class=\"c2\">\u0421\u0438\u0441\u0442\u0435\u043c\u044b \u0432\u043e\u043e\u0440\u0443\u0436\u0435\u043d\u0438\u044f: \u0423\u0434\u0430\u0440\u043d\u0438\u043a\u0438, \u043a\u043e\u043c\u043f\u043e\u043d\u0435\u043d\u0442\u044b \u0431\u0440\u043e\u043d\u0435\u0442\u0435\u0445\u043d\u0438\u043a\u0438.<\/span><\/li>\n\n<li><span class=\"c2\">\u0411\u0430\u043b\u043b\u0438\u0441\u0442\u0438\u0447\u0435\u0441\u043a\u043e\u0435 \u043f\u0440\u0438\u043c\u0435\u043d\u0435\u043d\u0438\u0435: \u043b\u0435\u0433\u043a\u0430\u044f \u0431\u0440\u043e\u043d\u044f \u0441 \u0432\u044b\u0441\u043e\u043a\u043e\u0439 \u0443\u0434\u0430\u0440\u043e\u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u044c\u044e.<\/span><\/li><\/ul><p class=\"c4 wp-block-paragraph\"><span class=\"c28 c5\">4. \u042d\u043d\u0435\u0440\u0433\u0435\u0442\u0438\u043a\u0430 \u0438 \u043f\u0440\u043e\u043c\u044b\u0448\u043b\u0435\u043d\u043d\u043e\u0441\u0442\u044c<\/span><\/p><ul class=\"wp-block-list c14 lst-kix_div1jargs9e8-0 start\"><li><span class=\"c2\">\u042f\u0434\u0435\u0440\u043d\u044b\u0435 \u0440\u0435\u0430\u043a\u0442\u043e\u0440\u044b: \u0440\u043e\u0442\u043e\u0440\u044b \u0446\u0435\u043d\u0442\u0440\u0438\u0444\u0443\u0433 \u0434\u043b\u044f \u043e\u0431\u043e\u0433\u0430\u0449\u0435\u043d\u0438\u044f \u0443\u0440\u0430\u043d\u0430.<\/span><\/li>\n\n<li><span class=\"c2\">\u041d\u0435\u0444\u0442\u044c \u0438 \u0433\u0430\u0437: \u0441\u043a\u0432\u0430\u0436\u0438\u043d\u043d\u044b\u0435 \u0438\u043d\u0441\u0442\u0440\u0443\u043c\u0435\u043d\u0442\u044b (\u0431\u0443\u0440\u043e\u0432\u044b\u0435 \u043e\u043f\u0440\u0430\u0432\u043a\u0438, \u043a\u043b\u0430\u043f\u0430\u043d\u044b), \u0443\u0441\u0442\u043e\u0439\u0447\u0438\u0432\u044b\u0435 \u043a \u0441\u0435\u0440\u043e\u0432\u043e\u0434\u043e\u0440\u043e\u0434\u043d\u043e\u0439 \u043a\u043e\u0440\u0440\u043e\u0437\u0438\u0438.<\/span><\/li><\/ul><p class=\"c4 wp-block-paragraph\"><span class=\"c5 c28\">5. \u041c\u0435\u0434\u0438\u0446\u0438\u043d\u0441\u043a\u0430\u044f \u0438 \u0442\u043e\u0447\u043d\u0430\u044f \u0438\u043d\u0436\u0435\u043d\u0435\u0440\u0438\u044f<\/span><\/p><ul class=\"wp-block-list c14 lst-kix_a1b0pskcel84-0 start\"><li><span class=\"c2\">\u0425\u0438\u0440\u0443\u0440\u0433\u0438\u0447\u0435\u0441\u043a\u0438\u0435 \u0438\u043d\u0441\u0442\u0440\u0443\u043c\u0435\u043d\u0442\u044b: \u0431\u0438\u043e\u0441\u043e\u0432\u043c\u0435\u0441\u0442\u0438\u043c\u044b\u0435, \u043d\u0435\u043c\u0430\u0433\u043d\u0438\u0442\u043d\u044b\u0435 \u0441\u0432\u043e\u0439\u0441\u0442\u0432\u0430 \u0434\u043b\u044f \u0441\u043e\u0432\u043c\u0435\u0441\u0442\u0438\u043c\u043e\u0441\u0442\u0438 \u0441 \u041c\u0420\u0422.<\/span><\/li>\n\n<li><span class=\"c2\">\u0412\u044b\u0441\u043e\u043a\u043e\u044d\u0444\u0444\u0435\u043a\u0442\u0438\u0432\u043d\u044b\u0435 \u043f\u0440\u0443\u0436\u0438\u043d\u044b: \u0441\u043e\u0445\u0440\u0430\u043d\u044f\u044e\u0442 \u044d\u043b\u0430\u0441\u0442\u0438\u0447\u043d\u043e\u0441\u0442\u044c \u043f\u0440\u0438 \u043c\u043d\u043e\u0433\u043e\u043a\u0440\u0430\u0442\u043d\u043e\u0439 \u043d\u0430\u0433\u0440\u0443\u0437\u043a\u0435.<\/span><\/li><\/ul><p class=\"c4 wp-block-paragraph\"><span class=\"c28 c5\">6. \u0421\u043f\u043e\u0440\u0442\u0438\u0432\u043d\u044b\u0435 \u0438 \u043f\u043e\u0442\u0440\u0435\u0431\u0438\u0442\u0435\u043b\u044c\u0441\u043a\u0438\u0435 \u0442\u043e\u0432\u0430\u0440\u044b<\/span><\/p><ul class=\"wp-block-list c14 lst-kix_ud3ato67ar2h-0 start\"><li><span class=\"c2\">\u0412\u0435\u043b\u043e\u0441\u0438\u043f\u0435\u0434\u044b \u0432\u044b\u0441\u0448\u0435\u0433\u043e \u043a\u043b\u0430\u0441\u0441\u0430: \u0440\u0430\u043c\u044b (\u043d\u0430\u043f\u0440\u0438\u043c\u0435\u0440, Reynolds 953) \u0434\u043b\u044f \u0434\u043e\u043b\u0433\u043e\u0432\u0435\u0447\u043d\u043e\u0441\u0442\u0438 \u0438 \u044d\u043a\u043e\u043d\u043e\u043c\u0438\u0438 \u0432\u0435\u0441\u0430.<\/span><\/li>\n\n<li><span class=\"c2\">\u041a\u043b\u044e\u0448\u043a\u0438 \u0434\u043b\u044f \u0433\u043e\u043b\u044c\u0444\u0430: \u0413\u043e\u043b\u043e\u0432\u043a\u0438 \u043a\u043b\u044e\u0448\u0435\u043a \u043e\u043f\u0442\u0438\u043c\u0438\u0437\u0438\u0440\u043e\u0432\u0430\u043d\u044b \u0434\u043b\u044f \u043e\u0431\u0435\u0441\u043f\u0435\u0447\u0435\u043d\u0438\u044f \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u0438 \u0438 \u0443\u0434\u0430\u0440\u043e\u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u0438.<\/span><\/li><\/ul><h2 class=\"wp-block-heading c4 c8\" id=\"h.drwqidqli630\"><span class=\"c26\">\u041a\u0430\u043a \u043f\u0440\u043e\u0438\u0437\u0432\u043e\u0434\u0438\u0442\u0441\u044f \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u043e-\u0441\u0442\u0430\u0440\u0435\u044e\u0449\u0430\u044f \u0441\u0442\u0430\u043b\u044c?<\/span><\/h2><p class=\"c4 wp-block-paragraph\"><span class=\"c2\">\u041c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u043e\u0441\u0442\u0430\u0440\u0435\u044e\u0449\u0430\u044f \u0441\u0442\u0430\u043b\u044c \u043f\u0440\u043e\u0438\u0437\u0432\u043e\u0434\u0438\u0442\u0441\u044f \u0432 \u0442\u0440\u0438 \u043e\u0441\u043d\u043e\u0432\u043d\u044b\u0445 \u044d\u0442\u0430\u043f\u0430:<\/span><\/p><ol start=\"1\" class=\"wp-block-list c14 lst-kix_8gl4x61d0ej1-0 start\"><li>\u041f\u043b\u0430\u0432\u043a\u0430 \u0441\u043f\u043b\u0430\u0432\u0430<span class=\"c2\">:<\/span><\/li><\/ol><p class=\"c4 wp-block-paragraph\"><span class=\"c2\">\u0412\u044b\u0441\u043e\u043a\u043e\u0447\u0438\u0441\u0442\u043e\u0435 \u0436\u0435\u043b\u0435\u0437\u043e, \u043d\u0438\u043a\u0435\u043b\u044c, \u043a\u043e\u0431\u0430\u043b\u044c\u0442 \u0438 \u0434\u0440\u0443\u0433\u0438\u0435 \u043c\u0435\u0442\u0430\u043b\u043b\u044b \u043f\u043b\u0430\u0432\u044f\u0442\u0441\u044f \u0432 \u0432\u0430\u043a\u0443\u0443\u043c\u0435 \u0434\u043b\u044f \u0443\u0434\u0430\u043b\u0435\u043d\u0438\u044f \u043f\u0440\u0438\u043c\u0435\u0441\u0435\u0439 \u0438 \u043e\u0431\u0435\u0441\u043f\u0435\u0447\u0435\u043d\u0438\u044f \u043e\u0434\u043d\u043e\u0440\u043e\u0434\u043d\u043e\u0441\u0442\u0438.<\/span><\/p><ol start=\"2\" class=\"wp-block-list c14 lst-kix_8gl4x61d0ej1-0\"><li>\u0422\u0435\u0440\u043c\u0438\u0447\u0435\u0441\u043a\u0430\u044f \u043e\u0431\u0440\u0430\u0431\u043e\u0442\u043a\u0430<span class=\"c2\">:<\/span><\/li><\/ol><p class=\"c4 wp-block-paragraph\">\u041e\u0442\u0436\u0438\u0433 \u0440\u0430\u0441\u0442\u0432\u043e\u0440\u0430<span class=\"c2\">: \u041d\u0430\u0433\u0440\u0435\u0432\u0430\u0435\u0442\u0441\u044f \u0434\u043b\u044f \u0440\u0430\u0441\u0442\u0432\u043e\u0440\u0435\u043d\u0438\u044f \u044d\u043b\u0435\u043c\u0435\u043d\u0442\u043e\u0432, \u0437\u0430\u0442\u0435\u043c \u043e\u0445\u043b\u0430\u0436\u0434\u0430\u0435\u0442\u0441\u044f \u0434\u043b\u044f \u0444\u043e\u0440\u043c\u0438\u0440\u043e\u0432\u0430\u043d\u0438\u044f \u043c\u044f\u0433\u043a\u043e\u0439, \u043f\u0440\u0438\u0433\u043e\u0434\u043d\u043e\u0439 \u0434\u043b\u044f \u043e\u0431\u0440\u0430\u0431\u043e\u0442\u043a\u0438 \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u043e\u0439 \u0441\u0442\u0440\u0443\u043a\u0442\u0443\u0440\u044b.<\/span><\/p><p class=\"c4 wp-block-paragraph\">\u0421\u0442\u0430\u0440\u0435\u043d\u0438\u0435<span class=\"c2\">: \u041d\u0430\u0433\u0440\u0435\u0432\u0430\u0435\u0442\u0441\u044f \u043f\u0440\u0438 \u0431\u043e\u043b\u0435\u0435 \u043d\u0438\u0437\u043a\u0438\u0445 \u0442\u0435\u043c\u043f\u0435\u0440\u0430\u0442\u0443\u0440\u0430\u0445 \u0434\u043b\u044f \u0441\u043e\u0437\u0434\u0430\u043d\u0438\u044f \u0432 \u0441\u0442\u0430\u043b\u0438 \u043c\u0435\u043b\u044c\u0447\u0430\u0439\u0448\u0438\u0445 \u0447\u0430\u0441\u0442\u0438\u0446, \u043f\u043e\u0432\u044b\u0448\u0430\u044e\u0449\u0438\u0445 \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u044c (\u043d\u0430\u043f\u0440\u0438\u043c\u0435\u0440, Ni\u2083Ti).<\/span><\/p><ol start=\"3\" class=\"wp-block-list c14 lst-kix_8gl4x61d0ej1-0\"><li>\u0424\u043e\u0440\u043c\u043e\u0432\u043a\u0430 \u0438 \u043e\u0442\u0434\u0435\u043b\u043a\u0430<span class=\"c2\">:<\/span><\/li><\/ol><p class=\"c4 wp-block-paragraph\"><span class=\"c2\">\u041b\u0435\u0433\u043a\u043e \u0444\u043e\u0440\u043c\u0443\u0435\u0442\u0441\u044f (\u043f\u0440\u043e\u043a\u0430\u0442\u044b\u0432\u0430\u0435\u0442\u0441\u044f, \u043a\u0443\u0435\u0442\u0441\u044f \u0438\u043b\u0438 \u043e\u0431\u0440\u0430\u0431\u0430\u0442\u044b\u0432\u0430\u0435\u0442\u0441\u044f) \u043f\u043e\u043a\u0430 \u043c\u044f\u0433\u043a\u0438\u0439. \u041f\u043e\u0441\u043b\u0435 \u0441\u0442\u0430\u0440\u0435\u043d\u0438\u044f \u0434\u043e\u043f\u043e\u043b\u043d\u0438\u0442\u0435\u043b\u044c\u043d\u0430\u044f \u043e\u0431\u0440\u0430\u0431\u043e\u0442\u043a\u0430 \u043f\u043e\u0432\u0435\u0440\u0445\u043d\u043e\u0441\u0442\u0438 (\u043d\u0430\u043f\u0440\u0438\u043c\u0435\u0440, \u0430\u0437\u043e\u0442\u0438\u0440\u043e\u0432\u0430\u043d\u0438\u0435) \u043f\u043e\u0432\u044b\u0448\u0430\u0435\u0442 \u0438\u0437\u043d\u043e\u0441\u043e\u0441\u0442\u043e\u0439\u043a\u043e\u0441\u0442\u044c.<\/span><\/p><p class=\"c4 wp-block-paragraph\"><span class=\"c2\">\u041c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u0430\u044f \u0441\u0442\u0430\u043b\u044c SteelPro Group \u043e\u0431\u0440\u0430\u0431\u0430\u0442\u044b\u0432\u0430\u0435\u0442\u0441\u044f \u043d\u0430 \u0441\u0442\u0430\u043d\u0435 \u0432 \u0442\u043e\u0447\u043d\u043e\u043c \u0441\u043e\u043e\u0442\u0432\u0435\u0442\u0441\u0442\u0432\u0438\u0438 \u0441 \u0432\u0430\u0448\u0438\u043c\u0438 \u0441\u043f\u0435\u0446\u0438\u0444\u0438\u043a\u0430\u0446\u0438\u044f\u043c\u0438, \u0447\u0442\u043e \u0441\u0432\u043e\u0434\u0438\u0442 \u043a \u043c\u0438\u043d\u0438\u043c\u0443\u043c\u0443 \u0437\u0430\u0434\u0435\u0440\u0436\u043a\u0438 \u043f\u043e\u0441\u043b\u0435 \u043e\u0431\u0440\u0430\u0431\u043e\u0442\u043a\u0438. \u041d\u0430\u0448\u0430 \u043a\u043e\u043c\u0430\u043d\u0434\u0430 \u043c\u043e\u0436\u0435\u0442 \u043e\u043f\u0442\u0438\u043c\u0438\u0437\u0438\u0440\u043e\u0432\u0430\u0442\u044c \u0432\u0430\u0448 \u0440\u0430\u0431\u043e\u0447\u0438\u0439 \u043f\u0440\u043e\u0446\u0435\u0441\u0441 \u043e\u0442 \u043f\u043b\u0430\u0432\u043a\u0438 \u0434\u043e \u0433\u043e\u0442\u043e\u0432\u043e\u0439 \u0434\u0435\u0442\u0430\u043b\u0438.<\/span><\/p><h2 class=\"wp-block-heading c4 c8\" id=\"h.jbm2u61t42rw\"><span class=\"c26\">\u0422\u0435\u0440\u043c\u043e\u043e\u0431\u0440\u0430\u0431\u043e\u0442\u043a\u0430 \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u043e\u0441\u0442\u0430\u0440\u0435\u044e\u0449\u0435\u0439 \u0441\u0442\u0430\u043b\u0438<\/span><\/h2><p class=\"c4 wp-block-paragraph\"><span class=\"c2\">\u041c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u0430\u044f \u0441\u0442\u0430\u043b\u044c \u0434\u043e\u0441\u0442\u0438\u0433\u0430\u0435\u0442 \u0441\u0432\u043e\u0438\u0445 \u0438\u0441\u043a\u043b\u044e\u0447\u0438\u0442\u0435\u043b\u044c\u043d\u044b\u0445 \u0441\u0432\u043e\u0439\u0441\u0442\u0432 \u043f\u043e\u0441\u0440\u0435\u0434\u0441\u0442\u0432\u043e\u043c \u043a\u043e\u043d\u0442\u0440\u043e\u043b\u0438\u0440\u0443\u0435\u043c\u043e\u0433\u043e \u043f\u0440\u043e\u0446\u0435\u0441\u0441\u0430 \u0442\u0435\u0440\u043c\u043e\u043e\u0431\u0440\u0430\u0431\u043e\u0442\u043a\u0438. \u0415\u0435 \u0441\u0432\u0435\u0440\u0445\u043d\u0438\u0437\u043a\u043e\u0435 \u0441\u043e\u0434\u0435\u0440\u0436\u0430\u043d\u0438\u0435 \u0443\u0433\u043b\u0435\u0440\u043e\u0434\u0430 (&lt;0,03%) \u043e\u0431\u0435\u0441\u043f\u0435\u0447\u0438\u0432\u0430\u0435\u0442 \u0433\u0438\u0431\u043a\u0443\u044e \u043e\u0431\u0440\u0430\u0431\u043e\u0442\u043a\u0443 \u0431\u0435\u0437 \u0445\u0440\u0443\u043f\u043a\u043e\u0441\u0442\u0438. \u041d\u0438\u0436\u0435 \u043f\u0440\u0438\u0432\u0435\u0434\u0435\u043d\u044b \u043e\u0441\u043d\u043e\u0432\u043d\u044b\u0435 \u044d\u0442\u0430\u043f\u044b:<\/span><\/p><h3 class=\"wp-block-heading c4 c8\" id=\"h.6t6fkn7eg4up\"><span class=\"c17\">\u041e\u0442\u0436\u0438\u0433 \u043d\u0430 \u0442\u0432\u0435\u0440\u0434\u044b\u0439 \u0440\u0430\u0441\u0442\u0432\u043e\u0440: \u043f\u043e\u0434\u0433\u043e\u0442\u043e\u0432\u043a\u0430 \u043e\u0441\u043d\u043e\u0432\u044b<\/span><\/h3><p class=\"c4 wp-block-paragraph\"><span class=\"c5\">\u041f\u0430\u0440\u0430\u043c\u0435\u0442\u0440\u044b \u043f\u0440\u043e\u0446\u0435\u0441\u0441\u0430<\/span><span class=\"c2\">:<\/span><\/p><ul class=\"wp-block-list c14 lst-kix_kwxf3invdz2u-0 start\"><li><span class=\"c5\">\u0422\u0435\u043c\u043f\u0435\u0440\u0430\u0442\u0443\u0440\u0430<\/span><span class=\"c2\">: 820\u00b0C (1510\u00b0F)<\/span><\/li>\n\n<li><span class=\"c5\">\u0412\u0440\u0435\u043c\u044f \u0437\u0430\u043c\u0430\u0447\u0438\u0432\u0430\u043d\u0438\u044f<\/span><span class=\"c2\">: 15 \u043c\u0438\u043d\u0443\u0442 \u0434\u043b\u044f \u0442\u043e\u043d\u043a\u0438\u0445 \u0441\u0440\u0435\u0437\u043e\u0432; 1 \u0447\u0430\u0441 \u043d\u0430 \u043a\u0430\u0436\u0434\u044b\u0435 25 \u043c\u043c (1 \u0434\u044e\u0439\u043c) \u0434\u043b\u044f \u0431\u043e\u043b\u0435\u0435 \u0442\u043e\u043b\u0441\u0442\u044b\u0445 \u0434\u0435\u0442\u0430\u043b\u0435\u0439.<\/span><\/li>\n\n<li><span class=\"c5\">\u041e\u0445\u043b\u0430\u0436\u0434\u0435\u043d\u0438\u0435<\/span><span class=\"c2\">: \u041e\u0445\u043b\u0430\u0436\u0434\u0435\u043d\u0438\u0435 \u043d\u0430 \u0432\u043e\u0437\u0434\u0443\u0445\u0435 \u0438\u043b\u0438 \u0437\u0430\u043a\u0430\u043b\u043a\u0430 \u0432 \u043c\u0430\u0441\u043b\u0435 \u0434\u043b\u044f \u043e\u0431\u0440\u0430\u0437\u043e\u0432\u0430\u043d\u0438\u044f \u043c\u044f\u0433\u043a\u043e\u0433\u043e \u043d\u0438\u0437\u043a\u043e\u0443\u0433\u043b\u0435\u0440\u043e\u0434\u0438\u0441\u0442\u043e\u0433\u043e \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u0430 (RC 30\u201335).<\/span><\/li><\/ul><p class=\"c4 wp-block-paragraph\"><span class=\"c5\">\u0420\u0435\u0437\u0443\u043b\u044c\u0442\u0430\u0442<\/span><span class=\"c2\">:<\/span><\/p><p class=\"c4 wp-block-paragraph\"><span class=\"c2\">\u0421\u0442\u0430\u043b\u044c \u0441\u0442\u0430\u043d\u043e\u0432\u0438\u0442\u0441\u044f \u043f\u043b\u0430\u0441\u0442\u0438\u0447\u043d\u043e\u0439 \u0438 \u043e\u0431\u0440\u0430\u0431\u0430\u0442\u044b\u0432\u0430\u0435\u043c\u043e\u0439, \u0441 \u0432\u044b\u0441\u043e\u043a\u043e\u0439 \u043f\u043b\u043e\u0442\u043d\u043e\u0441\u0442\u044c\u044e \u0434\u0438\u0441\u043b\u043e\u043a\u0430\u0446\u0438\u0439. \u042d\u0442\u043e\u0442 \u043f\u0440\u043e\u0446\u0435\u0441\u0441 \u0442\u0430\u043a\u0436\u0435 \u0441\u043d\u0438\u043c\u0430\u0435\u0442 \u043e\u0441\u0442\u0430\u0442\u043e\u0447\u043d\u044b\u0435 \u043d\u0430\u043f\u0440\u044f\u0436\u0435\u043d\u0438\u044f \u043e\u0442 \u043f\u0440\u0435\u0434\u044b\u0434\u0443\u0449\u0438\u0445 \u044d\u0442\u0430\u043f\u043e\u0432 \u043f\u0440\u043e\u0438\u0437\u0432\u043e\u0434\u0441\u0442\u0432\u0430, \u043e\u0431\u0435\u0441\u043f\u0435\u0447\u0438\u0432\u0430\u044f \u043b\u0443\u0447\u0448\u0443\u044e \u043f\u0440\u043e\u0438\u0437\u0432\u043e\u0434\u0438\u0442\u0435\u043b\u044c\u043d\u043e\u0441\u0442\u044c \u043d\u0430 \u043f\u043e\u0441\u043b\u0435\u0434\u0443\u044e\u0449\u0438\u0445 \u044d\u0442\u0430\u043f\u0430\u0445.<\/span><\/p><h3 class=\"wp-block-heading c4 c8\" id=\"h.d494it4ecrf6\"><span class=\"c17\">\u0421\u0442\u0430\u0440\u0435\u043d\u0438\u0435 (\u0434\u0438\u0441\u043f\u0435\u0440\u0441\u0438\u043e\u043d\u043d\u043e\u0435 \u0442\u0432\u0435\u0440\u0434\u0435\u043d\u0438\u0435): \u0432\u044b\u0441\u0432\u043e\u0431\u043e\u0436\u0434\u0435\u043d\u0438\u0435 \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u0438<\/span><\/h3><p class=\"c4 wp-block-paragraph\"><span class=\"c28 c5\">\u041f\u0440\u043e\u0446\u0435\u0441\u0441:<\/span><\/p><ul class=\"wp-block-list c14 lst-kix_xlo958iz671p-0 start\"><li><span class=\"c2\">\u041d\u0430\u0433\u0440\u0435\u0432 \u0434\u043e 480\u2013500\u00b0C (900\u2013930\u00b0F) \u043f\u0440\u0438\u0432\u043e\u0434\u0438\u0442 \u043a \u043e\u0431\u0440\u0430\u0437\u043e\u0432\u0430\u043d\u0438\u044e \u0441\u043e\u0435\u0434\u0438\u043d\u0435\u043d\u0438\u0439 \u0442\u0438\u043f\u0430 Ni\u2083Mo \u0438 Ni\u2083Ti. \u042d\u0442\u0438 \u0447\u0430\u0441\u0442\u0438\u0446\u044b \u0431\u043b\u043e\u043a\u0438\u0440\u0443\u044e\u0442 \u0434\u0432\u0438\u0436\u0435\u043d\u0438\u0435 \u0434\u0438\u0441\u043b\u043e\u043a\u0430\u0446\u0438\u0439, \u0443\u043f\u0440\u043e\u0447\u043d\u044f\u044f \u0441\u0442\u0430\u043b\u044c \u0431\u0435\u0437 \u043f\u043e\u0442\u0435\u0440\u0438 \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u0438.<\/span><\/li>\n\n<li><span class=\"c2\">\u0421\u0442\u0430\u043d\u0434\u0430\u0440\u0442\u043d\u0430\u044f \u043f\u0440\u043e\u0434\u043e\u043b\u0436\u0438\u0442\u0435\u043b\u044c\u043d\u043e\u0441\u0442\u044c \u0441\u0442\u0430\u0440\u0435\u043d\u0438\u044f \u0441\u043e\u0441\u0442\u0430\u0432\u043b\u044f\u0435\u0442 3 \u0447\u0430\u0441\u0430, \u043e\u0434\u043d\u0430\u043a\u043e \u0434\u043b\u044f \u0438\u0437\u0434\u0435\u043b\u0438\u0439 \u0441\u043b\u043e\u0436\u043d\u043e\u0439 \u0433\u0435\u043e\u043c\u0435\u0442\u0440\u0438\u0438 \u0435\u0435 \u043c\u043e\u0436\u043d\u043e \u0443\u0432\u0435\u043b\u0438\u0447\u0438\u0442\u044c \u0434\u043e 6 \u0447\u0430\u0441\u043e\u0432.<\/span><\/li>\n\n<li><span class=\"c2\">\u0415\u0441\u043b\u0438 \u0442\u0435\u043c\u043f\u0435\u0440\u0430\u0442\u0443\u0440\u0430 \u043f\u0440\u0435\u0432\u044b\u0448\u0430\u0435\u0442 500\u00b0C, \u043c\u043e\u0433\u0443\u0442 \u043e\u0431\u0440\u0430\u0437\u043e\u0432\u044b\u0432\u0430\u0442\u044c\u0441\u044f \u0433\u0440\u0443\u0431\u044b\u0435 \u0444\u0430\u0437\u044b, \u0442\u0430\u043a\u0438\u0435 \u043a\u0430\u043a Fe\u2082Mo, \u0447\u0442\u043e \u0441\u043d\u0438\u0436\u0430\u0435\u0442 \u043a\u0430\u043a \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u044c, \u0442\u0430\u043a \u0438 \u043f\u043b\u0430\u0441\u0442\u0438\u0447\u043d\u043e\u0441\u0442\u044c. \u0421\u0442\u0440\u043e\u0433\u0438\u0439 \u043a\u043e\u043d\u0442\u0440\u043e\u043b\u044c \u0442\u0435\u043c\u043f\u0435\u0440\u0430\u0442\u0443\u0440\u044b \u0438\u043c\u0435\u0435\u0442 \u0440\u0435\u0448\u0430\u044e\u0449\u0435\u0435 \u0437\u043d\u0430\u0447\u0435\u043d\u0438\u0435 \u0434\u043b\u044f \u043f\u0440\u0435\u0434\u043e\u0442\u0432\u0440\u0430\u0449\u0435\u043d\u0438\u044f \u044d\u0442\u0438\u0445 \u043d\u0435\u0433\u0430\u0442\u0438\u0432\u043d\u044b\u0445 \u044d\u0444\u0444\u0435\u043a\u0442\u043e\u0432.<\/span><\/li><\/ul><p class=\"c4 wp-block-paragraph\"><span class=\"c5\">\u0420\u0435\u0437\u0443\u043b\u044c\u0442\u0430\u0442<\/span><span class=\"c2\">:<\/span><\/p><p class=\"c4 wp-block-paragraph\">\u041f\u0440\u043e\u0446\u0435\u0441\u0441 \u0441\u0442\u0430\u0440\u0435\u043d\u0438\u044f \u0443\u0432\u0435\u043b\u0438\u0447\u0438\u0432\u0430\u0435\u0442 \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u044c \u0441\u0442\u0430\u043b\u0438, \u0434\u043e\u0441\u0442\u0438\u0433\u0430\u044f \u0434\u043e <span class=\"c5\">58 \u0427\u0420\u0421<\/span><span class=\"c2\">&nbsp;\u0434\u043b\u044f \u043c\u0430\u0440\u043a\u0438 C350. \u041f\u043e\u043b\u0443\u0447\u0435\u043d\u043d\u0430\u044f \u043c\u0438\u043a\u0440\u043e\u0441\u0442\u0440\u0443\u043a\u0442\u0443\u0440\u0430 \u0437\u043d\u0430\u0447\u0438\u0442\u0435\u043b\u044c\u043d\u043e \u043f\u043e\u0432\u044b\u0448\u0430\u0435\u0442 \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u044c \u043c\u0430\u0442\u0435\u0440\u0438\u0430\u043b\u0430, \u043d\u0435 \u0441\u043d\u0438\u0436\u0430\u044f \u0435\u0433\u043e \u0436\u0435\u0441\u0442\u043a\u043e\u0441\u0442\u0438, \u0447\u0442\u043e \u0434\u0435\u043b\u0430\u0435\u0442 \u0435\u0433\u043e \u0438\u0434\u0435\u0430\u043b\u044c\u043d\u044b\u043c \u0434\u043b\u044f \u0441\u043b\u043e\u0436\u043d\u044b\u0445 \u043f\u0440\u0438\u043c\u0435\u043d\u0435\u043d\u0438\u0439.<\/span><\/p><h3 class=\"wp-block-heading c8 c37\" id=\"h.qbmk3ftr74xx\">\u0423\u043b\u0443\u0447\u0448\u0435\u043d\u0438\u044f \u043f\u043e\u0441\u043b\u0435 \u043b\u0435\u0447\u0435\u043d\u0438\u044f<\/h3><p class=\"c4 wp-block-paragraph\"><span class=\"c5\">\u0410\u0437\u043e\u0442\u0438\u0440\u043e\u0432\u0430\u043d\u0438\u0435<\/span><span class=\"c2\">:<\/span><\/p><ul class=\"wp-block-list c14 lst-kix_ydcrq4dcelrm-0 start\"><li><span class=\"c5\">\u041f\u0440\u043e\u0446\u0435\u0441\u0441<\/span><span class=\"c2\">: \u0410\u0437\u043e\u0442 \u0434\u0438\u0444\u0444\u0443\u043d\u0434\u0438\u0440\u0443\u0435\u0442 \u0432 \u043f\u043e\u0432\u0435\u0440\u0445\u043d\u043e\u0441\u0442\u044c \u043f\u0440\u0438 \u0442\u0435\u043c\u043f\u0435\u0440\u0430\u0442\u0443\u0440\u0435 500\u2013550\u00b0C (930\u20131020\u00b0F).<\/span><\/li>\n\n<li><span class=\"c5\">\u0418\u0441\u0445\u043e\u0434<\/span><span class=\"c2\">: \u0422\u0432\u0435\u0440\u0434\u043e\u0441\u0442\u044c \u043f\u043e\u0432\u0435\u0440\u0445\u043d\u043e\u0441\u0442\u0438 \u0443\u0432\u0435\u043b\u0438\u0447\u0438\u0432\u0430\u0435\u0442\u0441\u044f \u0434\u043e \u0431\u043e\u043b\u0435\u0435 \u0447\u0435\u043c 60 HRC, \u0447\u0442\u043e \u0434\u0435\u043b\u0430\u0435\u0442 \u0435\u0435 \u0438\u0434\u0435\u0430\u043b\u044c\u043d\u043e\u0439 \u0434\u043b\u044f \u0438\u0437\u0433\u043e\u0442\u043e\u0432\u043b\u0435\u043d\u0438\u044f \u0438\u0437\u043d\u043e\u0441\u043e\u0441\u0442\u043e\u0439\u043a\u0438\u0445 \u0434\u0435\u0442\u0430\u043b\u0435\u0439, \u0442\u0430\u043a\u0438\u0445 \u043a\u0430\u043a \u0448\u0435\u0441\u0442\u0435\u0440\u043d\u0438.<\/span><\/li><\/ul><p class=\"c4 wp-block-paragraph\"><span class=\"c5\">\u0421\u043d\u044f\u0442\u0438\u0435 \u0441\u0442\u0440\u0435\u0441\u0441\u0430<\/span><span class=\"c2\">:<\/span><\/p><ul class=\"wp-block-list c14 lst-kix_rwznoor56j1s-0 start\"><li><span class=\"c5\">\u041f\u0440\u043e\u0446\u0435\u0441\u0441<\/span>: \u041e\u0442\u0436\u0438\u0433 \u043f\u0440\u0438 <span class=\"c5\">815\u2013830\u00b0C (1500\u20131525\u00b0F)<\/span><span class=\"c2\">\u00a0\u0438\u0437 \u0440\u0430\u0441\u0447\u0435\u0442\u0430 1 \u0447\u0430\u0441 \u043d\u0430 \u043a\u0430\u0436\u0434\u044b\u0439 \u0434\u044e\u0439\u043c \u0442\u043e\u043b\u0449\u0438\u043d\u044b.<\/span><\/li>\n\n<li><span class=\"c5\">\u0418\u0441\u0445\u043e\u0434<\/span>: <span class=\"c2\">\u0421\u043d\u044f\u0442\u0438\u0435 \u043d\u0430\u043f\u0440\u044f\u0436\u0435\u043d\u0438\u0439 \u043f\u043e\u043c\u043e\u0433\u0430\u0435\u0442 \u0432\u043e\u0441\u0441\u0442\u0430\u043d\u043e\u0432\u0438\u0442\u044c \u0441\u0432\u043e\u0439\u0441\u0442\u0432\u0430 \u043c\u0430\u0442\u0435\u0440\u0438\u0430\u043b\u0430 \u043f\u043e\u0441\u043b\u0435 \u0441\u0432\u0430\u0440\u043a\u0438 \u0438\u043b\u0438 \u0440\u0435\u043c\u043e\u043d\u0442\u0430. \u0418\u0441\u043f\u043e\u043b\u044c\u0437\u0443\u0435\u0442\u0441\u044f \u0434\u043b\u044f \u043e\u0442\u0440\u0435\u043c\u043e\u043d\u0442\u0438\u0440\u043e\u0432\u0430\u043d\u043d\u044b\u0445 \u0438\u043b\u0438 \u0441\u0432\u0430\u0440\u0435\u043d\u043d\u044b\u0445 \u0438\u043d\u0441\u0442\u0440\u0443\u043c\u0435\u043d\u0442\u043e\u0432 (\u043d\u0430\u043f\u0440\u0438\u043c\u0435\u0440, \u043b\u0438\u0442\u044c\u0435\u0432\u044b\u0445 \u0444\u043e\u0440\u043c).<\/span><\/li><\/ul><h2 class=\"wp-block-heading c4 c8\" id=\"h.8x7393kq5mfn\"><span class=\"c26\">\u041e\u0431\u0440\u0430\u0431\u043e\u0442\u043a\u0430 \u0438 \u043f\u0440\u043e\u0446\u0435\u0441\u0441 \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u043e\u0441\u0442\u0430\u0440\u0435\u044e\u0449\u0435\u0439 \u0441\u0442\u0430\u043b\u0438<\/span><\/h2><h3 class=\"wp-block-heading c13\" id=\"h.1l350za34cgl\"><span class=\"c17\">\u0425\u043e\u043b\u043e\u0434\u043d\u0430\u044f \u0438 \u0433\u043e\u0440\u044f\u0447\u0430\u044f \u043e\u0431\u0440\u0430\u0431\u043e\u0442\u043a\u0430<\/span><\/h3><p class=\"c4 wp-block-paragraph\">\u0412 \u043e\u0442\u043e\u0436\u0436\u0435\u043d\u043d\u043e\u043c \u0441\u043e\u0441\u0442\u043e\u044f\u043d\u0438\u0438 (RC 30\u201335) \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u043e\u0441\u0442\u0430\u0440\u0435\u044e\u0449\u0430\u044f \u0441\u0442\u0430\u043b\u044c \u043c\u043e\u0436\u0435\u0442 \u043f\u043e\u0434\u0432\u0435\u0440\u0433\u0430\u0442\u044c\u0441\u044f \u0445\u043e\u043b\u043e\u0434\u043d\u043e\u0439 \u043e\u0431\u0440\u0430\u0431\u043e\u0442\u043a\u0435 \u0441 \u0432\u043f\u0435\u0447\u0430\u0442\u043b\u044f\u044e\u0449\u0435\u0439 \u0433\u0438\u0431\u043a\u043e\u0441\u0442\u044c\u044e. \u0425\u043e\u043b\u043e\u0434\u043d\u0430\u044f \u043f\u0440\u043e\u043a\u0430\u0442\u043a\u0430 \u043c\u043e\u0436\u0435\u0442 \u0434\u043e\u0441\u0442\u0438\u0433\u0430\u0442\u044c <span class=\"c5\">90% \u0434\u0435\u0444\u043e\u0440\u043c\u0430\u0446\u0438\u044f<\/span><span class=\"c2\">&nbsp;\u0431\u0435\u0437 \u0442\u0440\u0435\u0449\u0438\u043d, \u0447\u0442\u043e \u0434\u0435\u043b\u0430\u0435\u0442 \u0435\u0433\u043e \u043f\u0440\u0438\u0433\u043e\u0434\u043d\u044b\u043c \u0434\u043b\u044f \u0442\u043e\u043d\u043a\u0438\u0445 \u043b\u0438\u0441\u0442\u043e\u0432 \u0438\u043b\u0438 \u043f\u0440\u0435\u0446\u0438\u0437\u0438\u043e\u043d\u043d\u043e\u0439 \u043f\u0440\u043e\u0432\u043e\u043b\u043e\u043a\u0438. <\/span><\/p><p class=\"c4 wp-block-paragraph\">\u0414\u043b\u044f \u0441\u043b\u043e\u0436\u043d\u044b\u0445 \u0444\u043e\u0440\u043c \u0433\u043e\u0440\u044f\u0447\u0430\u044f \u043e\u0431\u0440\u0430\u0431\u043e\u0442\u043a\u0430 \u043f\u0440\u0438 <span class=\"c5\">1000\u20131100\u00b0C (1832\u20132012\u00b0F)<\/span><span class=\"c2\">&nbsp;\u0441 \u043f\u043e\u0441\u043b\u0435\u0434\u0443\u044e\u0449\u0438\u043c \u0431\u044b\u0441\u0442\u0440\u044b\u043c \u043e\u0445\u043b\u0430\u0436\u0434\u0435\u043d\u0438\u0435\u043c \u0441\u043e\u0445\u0440\u0430\u043d\u044f\u0435\u0442 \u043f\u043b\u0430\u0441\u0442\u0438\u0447\u043d\u043e\u0441\u0442\u044c. \u041f\u043e\u0441\u043b\u0435 \u0444\u043e\u0440\u043c\u043e\u0432\u0430\u043d\u0438\u044f \u0441\u0442\u0430\u0440\u0435\u043d\u0438\u0435 \u0432\u043e\u0441\u0441\u0442\u0430\u043d\u0430\u0432\u043b\u0438\u0432\u0430\u0435\u0442 \u043f\u043e\u043b\u043d\u0443\u044e \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u044c. <\/span><\/p><p class=\"c4 wp-block-paragraph\"><span class=\"c2\">\u042d\u0442\u043e\u0442 \u043f\u0440\u043e\u0446\u0435\u0441\u0441 \u0438\u0434\u0435\u0430\u043b\u044c\u043d\u043e \u043f\u043e\u0434\u0445\u043e\u0434\u0438\u0442 \u0434\u043b\u044f \u043a\u0440\u0435\u043f\u0435\u0436\u043d\u044b\u0445 \u0434\u0435\u0442\u0430\u043b\u0435\u0439 \u0438 \u043a\u043e\u043d\u0441\u0442\u0440\u0443\u043a\u0442\u0438\u0432\u043d\u044b\u0445 \u044d\u043b\u0435\u043c\u0435\u043d\u0442\u043e\u0432 \u0432 \u0430\u044d\u0440\u043e\u043a\u043e\u0441\u043c\u0438\u0447\u0435\u0441\u043a\u043e\u0439 \u043e\u0442\u0440\u0430\u0441\u043b\u0438.<\/span><\/p><h3 class=\"wp-block-heading c13\" id=\"h.j87i8icpu8bu\"><span class=\"c17\">\u0421\u0432\u0430\u0440\u043a\u0430 \u0438 \u0441\u043e\u0435\u0434\u0438\u043d\u0435\u043d\u0438\u0435<\/span><\/h3><p class=\"c4 wp-block-paragraph\">\u041d\u0438\u0437\u043a\u043e\u0435 \u0441\u043e\u0434\u0435\u0440\u0436\u0430\u043d\u0438\u0435 \u0443\u0433\u043b\u0435\u0440\u043e\u0434\u0430 \u0432 \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u043e\u0441\u0442\u0430\u0440\u0435\u044e\u0449\u0435\u0439 \u0441\u0442\u0430\u043b\u0438 \u0443\u0441\u0442\u0440\u0430\u043d\u044f\u0435\u0442 \u043d\u0435\u043e\u0431\u0445\u043e\u0434\u0438\u043c\u043e\u0441\u0442\u044c \u043f\u0440\u0435\u0434\u0432\u0430\u0440\u0438\u0442\u0435\u043b\u044c\u043d\u043e\u0433\u043e \u043d\u0430\u0433\u0440\u0435\u0432\u0430, \u0447\u0442\u043e \u0443\u043f\u0440\u043e\u0449\u0430\u0435\u0442 \u043f\u0440\u043e\u0446\u0435\u0441\u0441 \u0441\u0432\u0430\u0440\u043a\u0438. <span class=\"c5\">TIG (\u0434\u0443\u0433\u043e\u0432\u0430\u044f \u0441\u0432\u0430\u0440\u043a\u0430 \u0432\u043e\u043b\u044c\u0444\u0440\u0430\u043c\u043e\u0432\u044b\u043c \u044d\u043b\u0435\u043a\u0442\u0440\u043e\u0434\u043e\u043c \u0432 \u0441\u0440\u0435\u0434\u0435 \u0438\u043d\u0435\u0440\u0442\u043d\u043e\u0433\u043e \u0433\u0430\u0437\u0430)<\/span>&nbsp;\u0438 <span class=\"c5\">\u043b\u0430\u0437\u0435\u0440\u043d\u0430\u044f \u0441\u0432\u0430\u0440\u043a\u0430<\/span><span class=\"c2\">&nbsp;\u044f\u0432\u043b\u044f\u044e\u0442\u0441\u044f \u043f\u0440\u0435\u0434\u043f\u043e\u0447\u0442\u0438\u0442\u0435\u043b\u044c\u043d\u044b\u043c\u0438 \u043c\u0435\u0442\u043e\u0434\u0430\u043c\u0438, \u043f\u043e\u0441\u043a\u043e\u043b\u044c\u043a\u0443 \u043e\u043d\u0438 \u043f\u0440\u0435\u0434\u043e\u0442\u0432\u0440\u0430\u0449\u0430\u044e\u0442 \u0437\u0430\u0433\u0440\u044f\u0437\u043d\u0435\u043d\u0438\u0435 \u0443\u0433\u043b\u0435\u0440\u043e\u0434\u043e\u043c. <\/span><\/p><p class=\"c4 wp-block-paragraph\">\u041f\u043e\u0441\u043b\u0435 \u0441\u0432\u0430\u0440\u043a\u0438 \u043a\u0440\u0430\u0439\u043d\u0435 \u0432\u0430\u0436\u043d\u043e <span class=\"c5\">\u043f\u043e\u0432\u0442\u043e\u0440\u043d\u043e\u0435 \u0441\u0442\u0430\u0440\u0435\u043d\u0438\u0435 \u0437\u043e\u043d\u044b \u0442\u0435\u0440\u043c\u0438\u0447\u0435\u0441\u043a\u043e\u0433\u043e \u0432\u043b\u0438\u044f\u043d\u0438\u044f (\u0417\u0422\u0412)<\/span><span class=\"c2\">&nbsp;\u043f\u0440\u0438 480\u2013500\u00b0C \u0432 \u0442\u0435\u0447\u0435\u043d\u0438\u0435 3 \u0447\u0430\u0441\u043e\u0432. \u042d\u0442\u043e\u0442 \u044d\u0442\u0430\u043f \u0443\u0434\u0430\u043b\u044f\u0435\u0442 \u043c\u044f\u0433\u043a\u0438\u0435 \u0437\u043e\u043d\u044b \u0438 \u043e\u0431\u0435\u0441\u043f\u0435\u0447\u0438\u0432\u0430\u0435\u0442 \u0440\u0430\u0432\u043d\u043e\u043c\u0435\u0440\u043d\u0443\u044e \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u044c, \u0447\u0442\u043e \u0438\u043c\u0435\u0435\u0442 \u0440\u0435\u0448\u0430\u044e\u0449\u0435\u0435 \u0437\u043d\u0430\u0447\u0435\u043d\u0438\u0435 \u0434\u043b\u044f \u0441\u043e\u0441\u0443\u0434\u043e\u0432 \u0432\u044b\u0441\u043e\u043a\u043e\u0433\u043e \u0434\u0430\u0432\u043b\u0435\u043d\u0438\u044f \u0438 \u043e\u0431\u043e\u0440\u043e\u043d\u043d\u043e\u0439 \u0442\u0435\u0445\u043d\u0438\u043a\u0438.<\/span><\/p><p class=\"c4 wp-block-paragraph\"><span class=\"c5\">\u041a\u043b\u044e\u0447\u0435\u0432\u044b\u0435 \u043f\u0430\u0440\u0430\u043c\u0435\u0442\u0440\u044b<\/span><span class=\"c2\">:<\/span><\/p><ul class=\"wp-block-list c14 lst-kix_571jg4nd1sea-0 start\"><li><span class=\"c2\">\u0417\u0430\u0449\u0438\u0442\u043d\u044b\u0439 \u0433\u0430\u0437: \u0430\u0440\u0433\u043e\u043d \u0438\u043b\u0438 \u0433\u0435\u043b\u0438\u0439 \u0434\u043b\u044f \u043f\u0440\u0435\u0434\u043e\u0442\u0432\u0440\u0430\u0449\u0435\u043d\u0438\u044f \u043e\u043a\u0438\u0441\u043b\u0435\u043d\u0438\u044f.<\/span><\/li>\n\n<li><span class=\"c2\">\u041f\u0440\u0438\u0441\u0430\u0434\u043e\u0447\u043d\u044b\u0439 \u043c\u0430\u0442\u0435\u0440\u0438\u0430\u043b: \u0441\u043e\u043e\u0442\u0432\u0435\u0442\u0441\u0442\u0432\u0443\u044e\u0449\u0438\u0439 \u0441\u043e\u0441\u0442\u0430\u0432 (\u043d\u0430\u043f\u0440\u0438\u043c\u0435\u0440, \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u0430\u044f \u043f\u0440\u043e\u0432\u043e\u043b\u043e\u043a\u0430 18Ni).<\/span><\/li><\/ul><h3 class=\"wp-block-heading c13\" id=\"h.9k211jpjetz1\"><span class=\"c17\">\u0410\u0434\u0434\u0438\u0442\u0438\u0432\u043d\u043e\u0435 \u043f\u0440\u043e\u0438\u0437\u0432\u043e\u0434\u0441\u0442\u0432\u043e (LPBF)<\/span><\/h3><p class=\"c4 wp-block-paragraph\"><span class=\"c2\">\u0422\u0435\u0445\u043d\u043e\u043b\u043e\u0433\u0438\u044f Laser Powder Bed Fusion (LPBF) \u043f\u0440\u0435\u043e\u0431\u0440\u0430\u0437\u0443\u0435\u0442 \u0438\u0441\u043f\u043e\u043b\u044c\u0437\u043e\u0432\u0430\u043d\u0438\u0435 \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u043e\u0439 \u0441\u0442\u0430\u043b\u0438 \u0432 \u043b\u0435\u0433\u043a\u0438\u0435, \u0432\u044b\u0441\u043e\u043a\u043e\u043f\u0440\u043e\u0447\u043d\u044b\u0435 \u043a\u043e\u043c\u043f\u043e\u043d\u0435\u043d\u0442\u044b. \u0412 \u044d\u0442\u043e\u043c \u043f\u0440\u043e\u0446\u0435\u0441\u0441\u0435 \u0442\u043e\u043d\u043a\u0438\u0439 \u043f\u043e\u0440\u043e\u0448\u043e\u043a \u0441\u043f\u043b\u0430\u0432\u0430 \u043f\u043b\u0430\u0432\u0438\u0442\u0441\u044f \u0441\u043b\u043e\u0439 \u0437\u0430 \u0441\u043b\u043e\u0435\u043c \u0441 \u043f\u043e\u043c\u043e\u0449\u044c\u044e \u043c\u043e\u0449\u043d\u043e\u0433\u043e \u043b\u0430\u0437\u0435\u0440\u0430.<\/span><\/p><p class=\"c4 wp-block-paragraph\"><span class=\"c5\">\u041e\u043f\u0442\u0438\u043c\u0438\u0437\u0438\u0440\u043e\u0432\u0430\u043d\u043d\u044b\u0439 \u0440\u0430\u0431\u043e\u0447\u0438\u0439 \u043f\u0440\u043e\u0446\u0435\u0441\u0441<\/span><span class=\"c2\">:<\/span><\/p><ol start=\"1\" class=\"wp-block-list c14 lst-kix_xl22b6kufpd5-0 start\"><li><span class=\"c5\">\u041f\u0435\u0447\u0430\u0442\u044c<\/span><span class=\"c2\">: \u041c\u043e\u0449\u043d\u043e\u0441\u0442\u044c \u043b\u0430\u0437\u0435\u0440\u0430 200\u2013400 \u0412\u0442, \u0441\u043a\u043e\u0440\u043e\u0441\u0442\u044c \u0441\u043a\u0430\u043d\u0438\u0440\u043e\u0432\u0430\u043d\u0438\u044f 800\u20131200 \u043c\u043c\/\u0441.<\/span><\/li>\n\n<li><span class=\"c5\">\u0421\u043d\u044f\u0442\u0438\u0435 \u0441\u0442\u0440\u0435\u0441\u0441\u0430<\/span><span class=\"c2\">: 600\u00b0C \u0432 \u0442\u0435\u0447\u0435\u043d\u0438\u0435 2 \u0447\u0430\u0441\u043e\u0432 \u0434\u043b\u044f \u0441\u043d\u0438\u0436\u0435\u043d\u0438\u044f \u043e\u0441\u0442\u0430\u0442\u043e\u0447\u043d\u044b\u0445 \u043d\u0430\u043f\u0440\u044f\u0436\u0435\u043d\u0438\u0439.<\/span><\/li>\n\n<li><span class=\"c5\">\u0421\u0442\u0430\u0440\u0435\u043d\u0438\u0435<\/span><span class=\"c2\">: \u0421\u0442\u0430\u043d\u0434\u0430\u0440\u0442\u043d\u0430\u044f \u043e\u0431\u0440\u0430\u0431\u043e\u0442\u043a\u0430 \u043f\u0440\u0438 480\u00b0C \u043f\u043e\u0432\u044b\u0448\u0430\u0435\u0442 \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u044c \u043d\u0430 30\u201340%.<\/span><\/li><\/ol><p class=\"c4 wp-block-paragraph\"><span class=\"c2\">\u041f\u043e\u0441\u0442\u043e\u0431\u0440\u0430\u0431\u043e\u0442\u043a\u0430, \u043d\u0430\u043f\u0440\u0438\u043c\u0435\u0440, \u0433\u043e\u0440\u044f\u0447\u0435\u0435 \u0438\u0437\u043e\u0441\u0442\u0430\u0442\u0438\u0447\u0435\u0441\u043a\u043e\u0435 \u043f\u0440\u0435\u0441\u0441\u043e\u0432\u0430\u043d\u0438\u0435 (HIP), \u043c\u043e\u0436\u0435\u0442 \u0434\u043e\u043f\u043e\u043b\u043d\u0438\u0442\u0435\u043b\u044c\u043d\u043e \u0443\u043b\u0443\u0447\u0448\u0438\u0442\u044c \u043f\u043b\u043e\u0442\u043d\u043e\u0441\u0442\u044c \u0438 \u0443\u0441\u0442\u0430\u043b\u043e\u0441\u0442\u043d\u0443\u044e \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u044c. \u042d\u0442\u043e\u0442 \u043c\u0435\u0442\u043e\u0434 \u043e\u0441\u043e\u0431\u0435\u043d\u043d\u043e \u0446\u0435\u043d\u0435\u043d \u0434\u043b\u044f \u0442\u0430\u043a\u0438\u0445 \u0434\u0435\u0442\u0430\u043b\u0435\u0439, \u043a\u0430\u043a \u043a\u0440\u043e\u043d\u0448\u0442\u0435\u0439\u043d\u044b \u0441\u043f\u0443\u0442\u043d\u0438\u043a\u043e\u0432 \u0438 \u0438\u043d\u0434\u0438\u0432\u0438\u0434\u0443\u0430\u043b\u044c\u043d\u044b\u0435 \u043c\u0435\u0434\u0438\u0446\u0438\u043d\u0441\u043a\u0438\u0435 \u0438\u043c\u043f\u043b\u0430\u043d\u0442\u0430\u0442\u044b, \u0433\u0434\u0435 \u0432\u0430\u0436\u043d\u044b \u0441\u043b\u043e\u0436\u043d\u044b\u0435 \u0433\u0435\u043e\u043c\u0435\u0442\u0440\u0438\u0438.<\/span><\/p><h3 class=\"wp-block-heading c13\" id=\"h.7t0u8jikfmpu\"><span class=\"c17\">\u0418\u043d\u0442\u0435\u043d\u0441\u0438\u0432\u043d\u0430\u044f \u043f\u043b\u0430\u0441\u0442\u0438\u0447\u0435\u0441\u043a\u0430\u044f \u0434\u0435\u0444\u043e\u0440\u043c\u0430\u0446\u0438\u044f (\u0418\u041f\u0414)<\/span><\/h3><p class=\"c4 wp-block-paragraph\">\u0414\u043b\u044f \u043f\u0440\u0438\u043c\u0435\u043d\u0435\u043d\u0438\u0439, \u0442\u0440\u0435\u0431\u0443\u044e\u0449\u0438\u0445 \u0447\u0440\u0435\u0437\u0432\u044b\u0447\u0430\u0439\u043d\u043e\u0439 \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u0438, \u043f\u0440\u0438\u043c\u0435\u043d\u044f\u044e\u0442\u0441\u044f \u0442\u0430\u043a\u0438\u0435 \u043c\u0435\u0442\u043e\u0434\u044b SPD, \u043a\u0430\u043a <span class=\"c5\">\u041a\u0440\u0443\u0447\u0435\u043d\u0438\u0435 \u043f\u043e\u0434 \u0432\u044b\u0441\u043e\u043a\u0438\u043c \u0434\u0430\u0432\u043b\u0435\u043d\u0438\u0435\u043c (HPT)<\/span>&nbsp;\u0438\u043b\u0438 <span class=\"c5\">\u0420\u0430\u0432\u043d\u043e\u043a\u0430\u043d\u0430\u043b\u044c\u043d\u043e\u0435 \u0443\u0433\u043b\u043e\u0432\u043e\u0435 \u043f\u0440\u0435\u0441\u0441\u043e\u0432\u0430\u043d\u0438\u0435 (\u0420\u041a\u0423\u041f)<\/span>&nbsp;\u0438\u0441\u043f\u043e\u043b\u044c\u0437\u0443\u044e\u0442\u0441\u044f \u0434\u043b\u044f \u0443\u043b\u0443\u0447\u0448\u0435\u043d\u0438\u044f \u043c\u0438\u043a\u0440\u043e\u0441\u0442\u0440\u0443\u043a\u0442\u0443\u0440\u044b \u0441\u0442\u0430\u043b\u0438. \u042d\u0442\u0438 \u043f\u0440\u043e\u0446\u0435\u0441\u0441\u044b \u0441\u043e\u0437\u0434\u0430\u044e\u0442 \u0441\u0432\u0435\u0440\u0445\u043c\u0435\u043b\u043a\u0438\u0435 \u0437\u0435\u0440\u043d\u0430 (&lt;100 \u043d\u043c) \u0438 \u0434\u0438\u0441\u043b\u043e\u043a\u0430\u0446\u0438\u043e\u043d\u043d\u044b\u0435 \u0441\u0435\u0442\u0438, \u043f\u0440\u043e\u0434\u0432\u0438\u0433\u0430\u044f \u043f\u0440\u0435\u0434\u0435\u043b \u0442\u0435\u043a\u0443\u0447\u0435\u0441\u0442\u0438 \u0437\u0430 \u043f\u0440\u0435\u0434\u0435\u043b\u044b <span class=\"c5\">3,0 \u0413\u041f\u0430<\/span><span class=\"c2\">. <\/span><\/p><p class=\"c4 wp-block-paragraph\"><span class=\"c2\">\u041d\u0435\u0441\u043c\u043e\u0442\u0440\u044f \u043d\u0430 \u0432\u044b\u0441\u043e\u043a\u0443\u044e \u0441\u0442\u043e\u0438\u043c\u043e\u0441\u0442\u044c, \u0442\u0435\u0445\u043d\u043e\u043b\u043e\u0433\u0438\u044f SPD \u0438\u043c\u0435\u0435\u0442 \u0440\u0435\u0448\u0430\u044e\u0449\u0435\u0435 \u0437\u043d\u0430\u0447\u0435\u043d\u0438\u0435 \u0434\u043b\u044f \u0442\u0430\u043a\u0438\u0445 \u043f\u0440\u0438\u043c\u0435\u043d\u0435\u043d\u0438\u0439, \u043a\u0430\u043a \u0438\u0437\u0433\u043e\u0442\u043e\u0432\u043b\u0435\u043d\u0438\u0435 \u0431\u0440\u043e\u043d\u0438 \u0438 \u043a\u043e\u043c\u043f\u043e\u043d\u0435\u043d\u0442\u043e\u0432, \u043f\u043e\u0434\u0432\u0435\u0440\u0436\u0435\u043d\u043d\u044b\u0445 \u043c\u043d\u043e\u0433\u043e\u0446\u0438\u043a\u043b\u043e\u0432\u043e\u0439 \u0443\u0441\u0442\u0430\u043b\u043e\u0441\u0442\u0438, \u0432 \u043e\u0431\u043e\u0440\u043e\u043d\u043d\u044b\u0445 \u0441\u0438\u0441\u0442\u0435\u043c\u0430\u0445.<\/span><\/p><h2 class=\"wp-block-heading c4 c8\" id=\"h.7y89ln64976r\"><span class=\"c26\">\u041f\u043b\u044e\u0441\u044b \u0438 \u043c\u0438\u043d\u0443\u0441\u044b \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u043e\u0441\u0442\u0430\u0440\u0435\u044e\u0449\u0435\u0439 \u0441\u0442\u0430\u043b\u0438<\/span><\/h2><h3 class=\"wp-block-heading c37 c8\" id=\"h.265wjdsvuk2a\"><span class=\"c17\">\u041f\u0440\u0435\u0438\u043c\u0443\u0449\u0435\u0441\u0442\u0432\u0430 \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u043e\u0441\u0442\u0430\u0440\u0435\u044e\u0449\u0435\u0439 \u0441\u0442\u0430\u043b\u0438<\/span><\/h3><ul class=\"wp-block-list c14 lst-kix_owk3wn4abpur-0 start\"><li><span class=\"c2\">\u0411\u0430\u043b\u0430\u043d\u0441 \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u0438 \u0438 \u0432\u044f\u0437\u043a\u043e\u0441\u0442\u0438: \u043f\u0440\u0435\u0432\u043e\u0441\u0445\u043e\u0434\u0438\u0442 \u0438\u043d\u0441\u0442\u0440\u0443\u043c\u0435\u043d\u0442\u0430\u043b\u044c\u043d\u044b\u0435 \u0441\u0442\u0430\u043b\u0438 (\u043d\u0430\u043f\u0440\u0438\u043c\u0435\u0440, H13) \u0438 \u0442\u0438\u0442\u0430\u043d\u043e\u0432\u044b\u0435 \u0441\u043f\u043b\u0430\u0432\u044b, \u0438\u043c\u0435\u044f \u043f\u0440\u0435\u0434\u0435\u043b \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u0438 \u043d\u0430 \u0440\u0430\u0441\u0442\u044f\u0436\u0435\u043d\u0438\u0435 \u0434\u043e 3,5 \u0413\u041f\u0430 \u0438 \u0432\u044f\u0437\u043a\u043e\u0441\u0442\u044c \u0440\u0430\u0437\u0440\u0443\u0448\u0435\u043d\u0438\u044f \u0431\u043e\u043b\u0435\u0435 175 \u041c\u041f\u0430\u00b7\u043c\u00b9\u2044\u00b2.<\/span><\/li>\n\n<li><span class=\"c2\">\u041f\u0440\u043e\u0441\u0442\u043e\u0442\u0430 \u0438\u0437\u0433\u043e\u0442\u043e\u0432\u043b\u0435\u043d\u0438\u044f: \u043f\u043e\u0434\u0434\u0430\u0435\u0442\u0441\u044f \u0445\u043e\u043b\u043e\u0434\u043d\u043e\u0439 \u043e\u0431\u0440\u0430\u0431\u043e\u0442\u043a\u0435 (\u0434\u0435\u0444\u043e\u0440\u043c\u0430\u0446\u0438\u044f \u0434\u043e 90%), \u0441\u0432\u0430\u0440\u0438\u0432\u0430\u0435\u0442\u0441\u044f \u0431\u0435\u0437 \u043f\u0440\u0435\u0434\u0432\u0430\u0440\u0438\u0442\u0435\u043b\u044c\u043d\u043e\u0433\u043e \u043d\u0430\u0433\u0440\u0435\u0432\u0430 \u0438 \u043f\u043e\u043b\u0438\u0440\u0443\u0435\u0442\u0441\u044f \u0434\u043e \u0437\u0435\u0440\u043a\u0430\u043b\u044c\u043d\u043e\u0433\u043e \u0431\u043b\u0435\u0441\u043a\u0430.<\/span><\/li>\n\n<li><span class=\"c2\">\u0423\u0441\u0442\u043e\u0439\u0447\u0438\u0432\u043e\u0441\u0442\u044c \u043a \u0432\u043e\u0437\u0434\u0435\u0439\u0441\u0442\u0432\u0438\u044e \u043e\u043a\u0440\u0443\u0436\u0430\u044e\u0449\u0435\u0439 \u0441\u0440\u0435\u0434\u044b: \u0412\u044b\u0441\u043e\u043a\u0430\u044f \u0441\u0442\u043e\u0439\u043a\u043e\u0441\u0442\u044c \u043a \u0432\u043e\u0434\u043e\u0440\u043e\u0434\u043d\u043e\u043c\u0443 \u043e\u0445\u0440\u0443\u043f\u0447\u0438\u0432\u0430\u043d\u0438\u044e \u0438 \u043a\u043e\u0440\u0440\u043e\u0437\u0438\u043e\u043d\u043d\u043e\u043c\u0443 \u0440\u0430\u0441\u0442\u0440\u0435\u0441\u043a\u0438\u0432\u0430\u043d\u0438\u044e \u043f\u043e\u0434 \u043d\u0430\u043f\u0440\u044f\u0436\u0435\u043d\u0438\u0435\u043c.<\/span><\/li><\/ul><h3 class=\"wp-block-heading c37 c8\" id=\"h.kng9dqgnme0i\"><span class=\"c17\">\u041e\u0433\u0440\u0430\u043d\u0438\u0447\u0435\u043d\u0438\u044f \u043f\u043e \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u043e\u0441\u0442\u0430\u0440\u0435\u044e\u0449\u0435\u0439 \u0441\u0442\u0430\u043b\u0438<\/span><\/h3><ul class=\"wp-block-list c14 lst-kix_krte87fytrtp-0 start\"><li><span class=\"c2\">\u0412\u044b\u0441\u043e\u043a\u0430\u044f \u0441\u0442\u043e\u0438\u043c\u043e\u0441\u0442\u044c: \u043e\u0431\u0443\u0441\u043b\u043e\u0432\u043b\u0435\u043d\u0430 \u0441\u043e\u0434\u0435\u0440\u0436\u0430\u043d\u0438\u0435\u043c \u043d\u0438\u043a\u0435\u043b\u044f \u0438 \u043a\u043e\u0431\u0430\u043b\u044c\u0442\u0430, \u0447\u0442\u043e \u043e\u0433\u0440\u0430\u043d\u0438\u0447\u0438\u0432\u0430\u0435\u0442 \u0438\u0441\u043f\u043e\u043b\u044c\u0437\u043e\u0432\u0430\u043d\u0438\u0435 \u0432 \u043f\u0440\u043e\u0435\u043a\u0442\u0430\u0445 \u0441 \u043e\u0433\u0440\u0430\u043d\u0438\u0447\u0435\u043d\u043d\u044b\u043c \u0431\u044e\u0434\u0436\u0435\u0442\u043e\u043c.<\/span><\/li>\n\n<li><span class=\"c2\">\u0422\u0435\u043c\u043f\u0435\u0440\u0430\u0442\u0443\u0440\u043d\u044b\u0435 \u043f\u0440\u0435\u0434\u0435\u043b\u044b: \u043f\u0440\u043e\u0447\u043d\u043e\u0441\u0442\u044c \u0440\u0435\u0437\u043a\u043e \u0441\u043d\u0438\u0436\u0430\u0435\u0442\u0441\u044f \u043f\u0440\u0438 \u0442\u0435\u043c\u043f\u0435\u0440\u0430\u0442\u0443\u0440\u0435 \u0432\u044b\u0448\u0435 400\u00b0C \u0438\u0437-\u0437\u0430 \u0440\u0435\u0432\u0435\u0440\u0441\u0438\u0438 \u0430\u0443\u0441\u0442\u0435\u043d\u0438\u0442\u0430.<\/span><\/li>\n\n<li><span class=\"c2\">\u0421\u043b\u043e\u0436\u043d\u043e\u0441\u0442\u044c \u043e\u0431\u0440\u0430\u0431\u043e\u0442\u043a\u0438 \u043f\u043e\u0441\u043b\u0435 \u0441\u0442\u0430\u0440\u0435\u043d\u0438\u044f: \u0442\u0440\u0435\u0431\u0443\u044e\u0442\u0441\u044f \u0442\u0432\u0435\u0440\u0434\u043e\u0441\u043f\u043b\u0430\u0432\u043d\u044b\u0435 \u0438\u043d\u0441\u0442\u0440\u0443\u043c\u0435\u043d\u0442\u044b \u0434\u043b\u044f \u0437\u0430\u043a\u0430\u043b\u0435\u043d\u043d\u044b\u0445 \u0441\u043e\u0441\u0442\u043e\u044f\u043d\u0438\u0439 (RC 55+), \u0447\u0442\u043e \u0441\u043d\u0438\u0436\u0430\u0435\u0442 \u044d\u0444\u0444\u0435\u043a\u0442\u0438\u0432\u043d\u043e\u0441\u0442\u044c.<\/span><\/li><\/ul><h2 class=\"wp-block-heading c22\" id=\"h.dhtli9ea736o\"><span class=\"c26\">\u041e\u043f\u0442\u0438\u043c\u0438\u0437\u0438\u0440\u0443\u0439\u0442\u0435 \u0441\u0432\u043e\u0439 \u043f\u0440\u043e\u0435\u043a\u0442 \u0441 \u043f\u043e\u043c\u043e\u0449\u044c\u044e \u043f\u0440\u043e\u0432\u0435\u0440\u0435\u043d\u043d\u043e\u0433\u043e \u043e\u043f\u044b\u0442\u0430 \u0432 \u043e\u0431\u043b\u0430\u0441\u0442\u0438 \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u043e\u0441\u0442\u0430\u0440\u0435\u044e\u0449\u0435\u0439 \u0441\u0442\u0430\u043b\u0438<\/span><\/h2><p class=\"c4 wp-block-paragraph\">\u041e\u0431\u043b\u0430\u0434\u0430\u044f \u0431\u043e\u043b\u0435\u0435 \u0447\u0435\u043c 20-\u043b\u0435\u0442\u043d\u0438\u043c \u043e\u043f\u044b\u0442\u043e\u043c \u0440\u0435\u0448\u0435\u043d\u0438\u044f \u0441\u043b\u043e\u0436\u043d\u044b\u0445 \u0438\u043d\u0436\u0435\u043d\u0435\u0440\u043d\u044b\u0445 \u0437\u0430\u0434\u0430\u0447, \u043c\u044b \u0433\u0430\u0440\u0430\u043d\u0442\u0438\u0440\u0443\u0435\u043c, \u0447\u0442\u043e \u0432\u0430\u0448\u0438 \u043a\u043e\u043c\u043f\u043e\u043d\u0435\u043d\u0442\u044b \u0438\u0437 \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u043e\u0441\u0442\u0430\u0440\u0435\u044e\u0449\u0435\u0439 \u0441\u0442\u0430\u043b\u0438 \u0431\u0443\u0434\u0443\u0442 \u0441\u043e\u043e\u0442\u0432\u0435\u0442\u0441\u0442\u0432\u043e\u0432\u0430\u0442\u044c \u0441\u0442\u0430\u043d\u0434\u0430\u0440\u0442\u0430\u043c \u043f\u0440\u043e\u0438\u0437\u0432\u043e\u0434\u0438\u0442\u0435\u043b\u044c\u043d\u043e\u0441\u0442\u0438 \u0438 \u0434\u0430\u0436\u0435 \u043f\u0440\u0435\u0432\u0437\u043e\u0439\u0434\u0443\u0442 \u0438\u0445. <span class=\"c5\">\u0413\u0440\u0443\u043f\u043f\u0430 \u043a\u043e\u043c\u043f\u0430\u043d\u0438\u0439 SteelPro<\/span><span class=\"c2\">, \u043c\u044b \u0441\u043e\u0435\u0434\u0438\u043d\u044f\u0435\u043c \u043c\u0430\u0442\u0435\u0440\u0438\u0430\u043b\u043e\u0432\u0435\u0434\u0435\u043d\u0438\u0435 \u0441 \u0440\u0435\u0430\u043b\u044c\u043d\u044b\u043c\u0438 \u043f\u0440\u0438\u043b\u043e\u0436\u0435\u043d\u0438\u044f\u043c\u0438. \u041d\u0430\u0448\u0430 \u0441\u0435\u0440\u0442\u0438\u0444\u0438\u0446\u0438\u0440\u043e\u0432\u0430\u043d\u043d\u0430\u044f \u043a\u043e\u043c\u0430\u043d\u0434\u0430 \u043f\u0440\u0435\u0434\u043e\u0441\u0442\u0430\u0432\u043b\u044f\u0435\u0442 \u0440\u0435\u0448\u0435\u043d\u0438\u044f \u0434\u043b\u044f \u043a\u043e\u043d\u043a\u0440\u0435\u0442\u043d\u044b\u0445 \u043c\u0430\u0440\u043e\u043a, \u043e\u0442 \u044d\u043a\u043e\u043d\u043e\u043c\u0438\u0447\u0435\u0441\u043a\u0438 \u044d\u0444\u0444\u0435\u043a\u0442\u0438\u0432\u043d\u043e\u0433\u043e \u0438\u043d\u0441\u0442\u0440\u0443\u043c\u0435\u043d\u0442\u0430 C200 \u0434\u043e \u044d\u043a\u0441\u043f\u043e\u0440\u0442\u043d\u043e-\u0441\u043e\u0432\u043c\u0435\u0441\u0442\u0438\u043c\u044b\u0445 \u044f\u0434\u0435\u0440\u043d\u044b\u0445 \u043a\u043e\u043c\u043f\u043e\u043d\u0435\u043d\u0442\u043e\u0432 C350.<\/span><\/p><p class=\"c4 wp-block-paragraph\"><span class=\"c2\">\u0421\u0432\u044f\u0436\u0438\u0442\u0435\u0441\u044c \u0441 \u043d\u0430\u043c\u0438, \u0447\u0442\u043e\u0431\u044b \u0443\u0432\u0435\u0440\u0435\u043d\u043d\u043e \u043d\u0430\u0447\u0430\u0442\u044c \u0441\u0432\u043e\u0439 \u043f\u0440\u043e\u0435\u043a\u0442 \u0443\u0436\u0435 \u0441\u0435\u0433\u043e\u0434\u043d\u044f!<\/span><\/p><p class=\"wp-block-paragraph\">&nbsp;<\/p>","protected":false},"excerpt":{"rendered":"<p>\u0420\u0443\u043a\u043e\u0432\u043e\u0434\u0441\u0442\u0432\u043e \u043f\u043e \u043c\u0430\u0440\u0442\u0435\u043d\u0441\u0438\u0442\u043d\u043e\u0441\u0442\u0430\u0440\u0435\u044e\u0449\u0435\u0439 \u0441\u0442\u0430\u043b\u0438: \u0441\u043e\u0441\u0442\u0430\u0432, \u0441\u0442\u0430\u0440\u0435\u043d\u0438\u0435, \u043e\u0431\u0440\u0430\u0431\u043e\u0442\u043a\u0430, \u043f\u043b\u044e\u0441\u044b\/\u043c\u0438\u043d\u0443\u0441\u044b. SteelPro Group \u0440\u0435\u0448\u0430\u0435\u0442 \u0432\u0430\u0448\u0438 \u0432\u044b\u0441\u043e\u043a\u043e\u043d\u0430\u043f\u0440\u044f\u0436\u0435\u043d\u043d\u044b\u0435 \u0438\u043d\u0436\u0435\u043d\u0435\u0440\u043d\u044b\u0435 \u0437\u0430\u0434\u0430\u0447\u0438.<\/p>","protected":false},"author":1,"featured_media":21411,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_acf_changed":false,"_eb_attr":"","rank_math_lock_modified_date":false,"site-sidebar-layout":"default","site-content-layout":"","ast-site-content-layout":"","site-content-style":"default","site-sidebar-style":"default","ast-global-header-display":"","ast-banner-title-visibility":"","ast-main-header-display":"","ast-hfb-above-header-display":"","ast-hfb-below-header-display":"","ast-hfb-mobile-header-display":"","site-post-title":"","ast-breadcrumbs-content":"","ast-featured-img":"","footer-sml-layout":"","theme-transparent-header-meta":"","adv-header-id-meta":"","stick-header-meta":"","header-above-stick-meta":"","header-main-stick-meta":"","header-below-stick-meta":"","astra-migrate-meta-layouts":"default","ast-page-background-enabled":"default","ast-page-background-meta":{"desktop":{"background-color":"var(--ast-global-color-4)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"ast-content-background-meta":{"desktop":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"tablet":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""},"mobile":{"background-color":"var(--ast-global-color-5)","background-image":"","background-repeat":"repeat","background-position":"center center","background-size":"auto","background-attachment":"scroll","background-type":"","background-media":"","overlay-type":"","overlay-color":"","overlay-opacity":"","overlay-gradient":""}},"footnotes":""},"categories":[4308],"tags":[],"class_list":["post-21410","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-alloy-steel"],"acf":[],"_links":{"self":[{"href":"https:\/\/steelprogroup.com\/ru\/wp-json\/wp\/v2\/posts\/21410","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/steelprogroup.com\/ru\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/steelprogroup.com\/ru\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/steelprogroup.com\/ru\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/steelprogroup.com\/ru\/wp-json\/wp\/v2\/comments?post=21410"}],"version-history":[{"count":0,"href":"https:\/\/steelprogroup.com\/ru\/wp-json\/wp\/v2\/posts\/21410\/revisions"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/steelprogroup.com\/ru\/wp-json\/wp\/v2\/media\/21411"}],"wp:attachment":[{"href":"https:\/\/steelprogroup.com\/ru\/wp-json\/wp\/v2\/media?parent=21410"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/steelprogroup.com\/ru\/wp-json\/wp\/v2\/categories?post=21410"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/steelprogroup.com\/ru\/wp-json\/wp\/v2\/tags?post=21410"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}